General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 10.2 g/cm³ Show Material materials with Density of 10.2 g/cm³ | Typical for Molybdenum |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 324 GPa Show Material materials with Elastic modulus of 324 GPa | Typical for Molybdenum |
Elongation | 20.0 °C | 15 % Show Material materials with Elongation of 15 % | |
Elongation A50 | 20.0 °C | 10 - 18 % Show Material materials with Elongation A50 of 10 - 18 % | |
Hardness, Vickers, 10 | 20.0 °C | 205 - 280 [-] Show Material materials with Hardness, Vickers, 10 of 205 - 280 [-] | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Molybdenum |
Shear modulus | 23.0 °C | 125 GPa Show Material materials with Shear modulus of 125 GPa | Typical for Molybdenum |
Tensile strength | 20.0 °C | 450 - 620 MPa Show Material materials with Tensile strength of 450 - 620 MPa | |
Yield strength | 20.0 °C | 380 - 515 MPa Show Material materials with Yield strength of 380 - 515 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 4E-6 - 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 4E-6 - 1.4E-5 1/K | Typical for Molybdenum |
Melting point | 2610 °C Show Material materials with Melting point of 2610 °C | Typical for Molybdenum | |
Specific heat capacity | 23.0 °C | 201 - 280 J/(kg·K) Show Material materials with Specific heat capacity of 201 - 280 J/(kg·K) | Typical for Molybdenum |
Thermal conductivity | 23.0 °C | 117 - 431 W/(m·K) Show Material materials with Thermal conductivity of 117 - 431 W/(m·K) | Typical for Molybdenum |
Chemical properties
Property | Value |
---|---|
Carbon | 0.03 % Show Material materials with Carbon of 0.03 % |
Iron | 0.01 % Show Material materials with Iron of 0.01 % |
Nickel | 2E-3 % Show Material materials with Nickel of 2E-3 % |
Nitrogen | 2E-3 % Show Material materials with Nitrogen of 2E-3 % |
Oxygen | 1.5E-3 % Show Material materials with Oxygen of 1.5E-3 % |
Silicon | 0.01 % Show Material materials with Silicon of 0.01 % |