General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 6.51 g/cm³ Show Material materials with Density of 6.51 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 99.2 GPa Show Material materials with Elastic modulus of 99.2 GPa |
38.0 °C | 98.6 GPa Show Material materials with Elastic modulus of 98.6 GPa | |
93.0 °C | 93.1 GPa Show Material materials with Elastic modulus of 93.1 GPa | |
149.0 °C | 86.9 GPa Show Material materials with Elastic modulus of 86.9 GPa | |
204.0 °C | 80.7 GPa Show Material materials with Elastic modulus of 80.7 GPa | |
260.0 °C | 75.2 GPa Show Material materials with Elastic modulus of 75.2 GPa | |
316.0 °C | 69.6 GPa Show Material materials with Elastic modulus of 69.6 GPa | |
371.0 °C | 64.1 GPa Show Material materials with Elastic modulus of 64.1 GPa | |
Poisson's ratio | 20.0 °C | 0.35 [-] Show Material materials with Poisson's ratio of 0.35 [-] |
Shear modulus | 20.0 °C | 36.2 GPa Show Material materials with Shear modulus of 36.2 GPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 5.7E-6 - 7E-6 1/K Show Material materials with Coefficient of thermal expansion of 5.7E-6 - 7E-6 1/K | Typical for Zirconium |
Melting point | 1845 °C Show Material materials with Melting point of 1845 °C | Typical for Zirconium | |
Specific heat capacity | 100.0 °C | 284.7 J/(kg·K) Show Material materials with Specific heat capacity of 284.7 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 22 W/(m·K) Show Material materials with Thermal conductivity of 22 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbon | 0.05 % Show Material materials with Carbon of 0.05 % |
Hafnium | 4.5 % Show Material materials with Hafnium of 4.5 % |
Hydrogen | 4E-3 % Show Material materials with Hydrogen of 4E-3 % |
Nitrogen | 0.02 % Show Material materials with Nitrogen of 0.02 % |
Oxygen | 0.16 % Show Material materials with Oxygen of 0.16 % |