General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 6.64 g/cm³ Show Material materials with Density of 6.64 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 94.7 GPa Show Material materials with Elastic modulus of 94.7 GPa |
38.0 °C | 93.8 GPa Show Material materials with Elastic modulus of 93.8 GPa | |
93.0 °C | 90.5 GPa Show Material materials with Elastic modulus of 90.5 GPa | |
149.0 °C | 87.3 GPa Show Material materials with Elastic modulus of 87.3 GPa | |
204.0 °C | 84.2 GPa Show Material materials with Elastic modulus of 84.2 GPa | |
260.0 °C | 81 GPa Show Material materials with Elastic modulus of 81 GPa | |
316.0 °C | 77.8 GPa Show Material materials with Elastic modulus of 77.8 GPa | |
371.0 °C | 74.6 GPa Show Material materials with Elastic modulus of 74.6 GPa | |
Elongation A50 | 20.0 °C | 16 % Show Material materials with Elongation A50 of 16 % |
Poisson's ratio | 20.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] |
Shear modulus | 20.0 °C | 34.5 GPa Show Material materials with Shear modulus of 34.5 GPa |
Tensile strength | 20.0 °C | 550 MPa Show Material materials with Tensile strength of 550 MPa |
Yield strength Rp0.2 | 20.0 °C | 380 MPa Show Material materials with Yield strength Rp0.2 of 380 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 5.7E-6 - 7E-6 1/K Show Material materials with Coefficient of thermal expansion of 5.7E-6 - 7E-6 1/K | Typical for Zirconium |
Melting point | 1845 °C Show Material materials with Melting point of 1845 °C | Typical for Zirconium | |
Specific heat capacity | 100.0 °C | 280.5 J/(kg·K) Show Material materials with Specific heat capacity of 280.5 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 17.1 W/(m·K) Show Material materials with Thermal conductivity of 17.1 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbon | 0.05 % Show Material materials with Carbon of 0.05 % |
Hafnium | 4.5 % Show Material materials with Hafnium of 4.5 % |
Hydrogen | 5E-3 % Show Material materials with Hydrogen of 5E-3 % |
Niobium | 2 - 3 % Show Material materials with Niobium of 2 - 3 % |
Nitrogen | 0.03 % Show Material materials with Nitrogen of 0.03 % |
Oxygen | 0.16 % Show Material materials with Oxygen of 0.16 % |