ASTM B551 Grade R60702 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

Strip, sheet and plate from high corrosion resistant unalloyed zirconium.

Related Standards

Ashby charts

See where ASTM B551 Grade R60702 soft annealed (+A) falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

Density

ρ

6.51 g/cm³ at 20 °C

Mechanical

Elastic modulus

E

99.2 GPa at 20 °C

Show Zirconium materials with Elastic modulus of 99.2 GPa at 20 °C

Hide chart

Elongation A50

A50

16 % at 20 °C

Show Zirconium materials with Elongation A50 of 16 % at 20 °C

Poisson's ratio

ν

0.35 [-] at 20 °C

Show Zirconium materials with Poisson's ratio of 0.35 [-] at 20 °C

Shear modulus

G

36.2 GPa at 20 °C

Show Zirconium materials with Shear modulus of 36.2 GPa at 20 °C

Tensile strength

Rm

380 MPa at 20 °C

Show Zirconium materials with Tensile strength of 380 MPa at 20 °C

Yield strength Rp0.2

Rp0.2

205 MPa at 20 °C

Show Zirconium materials with Yield strength Rp0.2 of 205 MPa at 20 °C

Thermal

Coefficient of thermal expansion

α

5.7E-6 - 7E-6 1/K at 23 °C

Typical for Zirconium

Melting point

Tm

1845 °C

Typical for Zirconium

Specific heat capacity

cp

284.7 J/(kg·K) at 100 °C

Thermal conductivity

λ

22 W/(m·K) at 20 °C

Chemical properties

Element

Weight %

Comment

Hf

4.5 %

O

0.16 %

C

0.05 %

N

0.03 %

H

5E-3 %

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.