Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.53 g/cm³ Show Supplier Material materials with Dichte of 1.53 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Wasserabsorption | 4.4 % Show Supplier Material materials with Wasserabsorption of 4.4 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 13.5 GPa Show Supplier Material materials with Biegemodul of 13.5 GPa | dry | ISO 178 | |
Dehnung | 2 % Show Supplier Material materials with Dehnung of 2 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 13.5 GPa Show Supplier Material materials with Elastizitätsmodul of 13.5 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 330 MPa Show Supplier Material materials with Flexural yield strength of 330 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | dry | ISO 179/1eA |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 65 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 65 kJ/m² | dry | ISO 179/1eU |
Zugfestigkeit | 210 MPa Show Supplier Material materials with Zugfestigkeit of 210 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 125 °C Show Supplier Material materials with Glasübergangstemperatur of 125 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 3e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3e-07 1/K | dry | ASTM D696 | Parallel | |
4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4e-07 1/K | dry | ASTM D696 | Normal | ||
Schmelzpunkt | 325 °C Show Supplier Material materials with Schmelzpunkt of 325 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 305 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 305 °C | dry | ISO 75-1/-2 | 2 MPa | |
320 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 320 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | dry, conditioned | IEC 62631-2-1 | 1MHz |
5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 5 [-] | dry, conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 33 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 33 kV/mm | dry, conditioned | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 120 [-] Show Supplier Material materials with Verlustfaktor of 120 [-] | dry, conditioned | IEC 62631-2-1 | 100Hz |
250 [-] Show Supplier Material materials with Verlustfaktor of 250 [-] | dry, conditioned | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Reflow connectors (3) | |
Certifications | Yellow Card Available | |
Fillers | 40% Glass Fiber |