Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.62 g/cm³ Show Supplier Material materials with Dichte of 1.62 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.6 % Show Supplier Material materials with Moisture absorption of 1.6 % | dry | Sim. to ISO 62 |
Wasserabsorption | 3.4 % Show Supplier Material materials with Wasserabsorption of 3.4 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 17 GPa Show Supplier Material materials with Biegemodul of 17 GPa | dry | ISO 178 | |
17.8 GPa Show Supplier Material materials with Biegemodul of 17.8 GPa | conditioned | ISO 178 | ||
120 °C | 16.5 GPa Show Supplier Material materials with Biegemodul of 16.5 GPa | dry | ISO 178 | |
160 °C | 6.3 GPa Show Supplier Material materials with Biegemodul of 6.3 GPa | dry | ISO 178 | |
180 °C | 5 GPa Show Supplier Material materials with Biegemodul of 5 GPa | dry | ISO 178 | |
200 °C | 4.7 GPa Show Supplier Material materials with Biegemodul of 4.7 GPa | dry | ISO 178 | |
210 °C | 4.5 GPa Show Supplier Material materials with Biegemodul of 4.5 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2.8 % Show Supplier Material materials with Dehnung of 2.8 % | dry | ISO 527-1/-2 |
2.3 % Show Supplier Material materials with Dehnung of 2.3 % | conditioned | ISO 527-1/-2 | ||
2.5 % Show Supplier Material materials with Dehnung of 2.5 % | dry | ISO 527-1/-2 | ||
40 °C | 2.5 % Show Supplier Material materials with Dehnung of 2.5 % | dry | ISO 527-1/-2 | |
80 °C | 2.5 % Show Supplier Material materials with Dehnung of 2.5 % | dry | ISO 527-1/-2 | |
80 °C | 5 % Show Supplier Material materials with Dehnung of 5 % | conditioned | ISO 527-1/-2 | |
100 °C | 2.7 % Show Supplier Material materials with Dehnung of 2.7 % | dry | ISO 527-1/-2 | |
100 °C | 8 % Show Supplier Material materials with Dehnung of 8 % | conditioned | ISO 527-1/-2 | |
120 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 | |
120 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | conditioned | ISO 527-1/-2 | |
150 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | dry | ISO 527-1/-2 | |
160 °C | 10 % Show Supplier Material materials with Dehnung of 10 % | dry | ISO 527-1/-2 | |
180 °C | 9 % Show Supplier Material materials with Dehnung of 9 % | dry | ISO 527-1/-2 | |
200 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | dry | ISO 527-1/-2 | |
210 °C | 0.006 % Show Supplier Material materials with Dehnung of 0.006 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 17.5 GPa Show Supplier Material materials with Elastizitätsmodul of 17.5 GPa | dry | ISO 527-1/-2 |
17.5 GPa Show Supplier Material materials with Elastizitätsmodul of 17.5 GPa | dry | ISO 527-1/-2 | ||
18 GPa Show Supplier Material materials with Elastizitätsmodul of 18 GPa | conditioned | ISO 527-1/-2 | ||
40 °C | 17 GPa Show Supplier Material materials with Elastizitätsmodul of 17 GPa | dry | ISO 527-1/-2 | |
80 °C | 13.5 GPa Show Supplier Material materials with Elastizitätsmodul of 13.5 GPa | conditioned | ISO 527-1/-2 | |
80 °C | 16.5 GPa Show Supplier Material materials with Elastizitätsmodul of 16.5 GPa | dry | ISO 527-1/-2 | |
100 °C | 5.7 GPa Show Supplier Material materials with Elastizitätsmodul of 5.7 GPa | conditioned | ISO 527-1/-2 | |
100 °C | 15.9 GPa Show Supplier Material materials with Elastizitätsmodul of 15.9 GPa | dry | ISO 527-1/-2 | |
120 °C | 5.1 GPa Show Supplier Material materials with Elastizitätsmodul of 5.1 GPa | conditioned | ISO 527-1/-2 | |
120 °C | 14.5 GPa Show Supplier Material materials with Elastizitätsmodul of 14.5 GPa | dry | ISO 527-1/-2 | |
150 °C | 7.4 GPa Show Supplier Material materials with Elastizitätsmodul of 7.4 GPa | dry | ISO 527-1/-2 | |
160 °C | 5.3 GPa Show Supplier Material materials with Elastizitätsmodul of 5.3 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.5 GPa Show Supplier Material materials with Elastizitätsmodul of 4.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 3.9 GPa Show Supplier Material materials with Elastizitätsmodul of 3.9 GPa | dry | ISO 527-1/-2 | |
210 °C | 3.8 GPa Show Supplier Material materials with Elastizitätsmodul of 3.8 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 370 MPa Show Supplier Material materials with Flexural yield strength of 370 MPa | conditioned | ISO 178 | |
410 MPa Show Supplier Material materials with Flexural yield strength of 410 MPa | dry | ISO 178 | ||
120 °C | 280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 10 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 12 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12 kJ/m² | dry | ISO 179/1eA | |
23 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 12.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12.5 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | dry | ISO 179/1eU | |
23 °C | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 330 MPa Show Supplier Material materials with Zugfestigkeit of 330 MPa | dry | ISO 527-1/-2 |
250 MPa Show Supplier Material materials with Zugfestigkeit of 250 MPa | conditioned | ISO 527-1/-2 | ||
270 MPa Show Supplier Material materials with Zugfestigkeit of 270 MPa | dry | ISO 527-1/-2 | ||
40 °C | 255 MPa Show Supplier Material materials with Zugfestigkeit of 255 MPa | dry | ISO 527-1/-2 | |
80 °C | 115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 205 MPa Show Supplier Material materials with Zugfestigkeit of 205 MPa | dry | ISO 527-1/-2 | |
100 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | conditioned | ISO 527-1/-2 | |
100 °C | 185 MPa Show Supplier Material materials with Zugfestigkeit of 185 MPa | dry | ISO 527-1/-2 | |
120 °C | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | conditioned | ISO 527-1/-2 | |
120 °C | 150 MPa Show Supplier Material materials with Zugfestigkeit of 150 MPa | dry | ISO 527-1/-2 | |
150 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |
160 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | dry | ISO 527-1/-2 | |
180 °C | 55.0 MPa Show Supplier Material materials with Zugfestigkeit of 55.0 MPa | dry | ISO 527-1/-2 | |
200 °C | 42 MPa Show Supplier Material materials with Zugfestigkeit of 42 MPa | dry | ISO 527-1/-2 | |
210 °C | 40 MPa Show Supplier Material materials with Zugfestigkeit of 40 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Glasübergangstemperatur | 150 °C Show Supplier Material materials with Glasübergangstemperatur of 150 °C | dry | ASTM D5026/D7028 | DMTA (tan d) | ||
Glow Wire Flammability Index | 700 °C Show Supplier Material materials with Glow Wire Flammability Index of 700 °C | dry | IEC 60695-2-12 | 2 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | |||
Glow Wire Ignition Temperature | 725 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 725 °C | dry | IEC 60695-2-13 | 2 mm | ||
800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | dry | IEC 60695-2-13 | 3 mm | |||
Koeffizient der thermischen Ausdehnung | 2.7e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2.7e-07 1/K | dry | ASTM D696 | Parallel | ||
2.9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2.9e-07 1/K | dry | ASTM D696 | Normal | |||
Schmelzpunkt | 320 °C Show Supplier Material materials with Schmelzpunkt of 320 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 275 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 275 °C | dry | ISO 75-1/-2 | 2 MPa | ||
302 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 302 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4.9 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.9 [-] | dry | IEC 62631-2-1 | 1MHz |
5.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 5.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 19 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 19 kV/mm | conditioned | IEC 60243-1 | |
20 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 20 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 425 V Show Supplier Material materials with Kriechstromfestigkeit of 425 V | dry | IEC 60112 | |
Surface resistivity | 4e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 4e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 | ||
Verlustfaktor | 90 [-] Show Supplier Material materials with Verlustfaktor of 90 [-] | dry | IEC 62631-2-1 | 100Hz |
190 [-] Show Supplier Material materials with Verlustfaktor of 190 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Structural Parts with ForTii® Ace, Demo structural part | |
Fillers | 50% Glass Fiber |