Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.56 g/cm³ Show Supplier Material materials with Dichte of 1.56 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | dry | Sim. to ISO 62 |
Wasserabsorption | 4.5 % Show Supplier Material materials with Wasserabsorption of 4.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 10.5 GPa Show Supplier Material materials with Biegemodul of 10.5 GPa | conditioned | ISO 178 | |
16.5 GPa Show Supplier Material materials with Biegemodul of 16.5 GPa | dry | ISO 178 | ||
120 °C | 7.8 GPa Show Supplier Material materials with Biegemodul of 7.8 GPa | dry | ISO 178 | |
160 °C | 6.9 GPa Show Supplier Material materials with Biegemodul of 6.9 GPa | dry | ISO 178 | |
180 °C | 6.4 GPa Show Supplier Material materials with Biegemodul of 6.4 GPa | dry | ISO 178 | |
200 °C | 5.6 GPa Show Supplier Material materials with Biegemodul of 5.6 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2.7 % Show Supplier Material materials with Dehnung of 2.7 % | dry | ISO 527-1/-2 |
2.7 % Show Supplier Material materials with Dehnung of 2.7 % | dry | ISO 527-1/-2 | ||
5 % Show Supplier Material materials with Dehnung of 5 % | conditioned | ISO 527-1/-2 | ||
120 °C | 6.4 % Show Supplier Material materials with Dehnung of 6.4 % | dry | ISO 527-1/-2 | |
150 °C | 6.4 % Show Supplier Material materials with Dehnung of 6.4 % | dry | ISO 527-1/-2 | |
160 °C | 6.5 % Show Supplier Material materials with Dehnung of 6.5 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 17 GPa Show Supplier Material materials with Elastizitätsmodul of 17 GPa | dry | ISO 527-1/-2 |
11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | conditioned | ISO 527-1/-2 | ||
16.5 GPa Show Supplier Material materials with Elastizitätsmodul of 16.5 GPa | dry | ISO 527-1/-2 | ||
40 °C | 14.7 GPa Show Supplier Material materials with Elastizitätsmodul of 14.7 GPa | dry | ISO 527-1/-2 | |
100 °C | 7.2 GPa Show Supplier Material materials with Elastizitätsmodul of 7.2 GPa | dry | ISO 527-1/-2 | |
120 °C | 6.8 GPa Show Supplier Material materials with Elastizitätsmodul of 6.8 GPa | dry | ISO 527-1/-2 | |
150 °C | 6 GPa Show Supplier Material materials with Elastizitätsmodul of 6 GPa | dry | ISO 527-1/-2 | |
160 °C | 5.6 GPa Show Supplier Material materials with Elastizitätsmodul of 5.6 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 240 MPa Show Supplier Material materials with Flexural yield strength of 240 MPa | conditioned | ISO 178 | |
370 MPa Show Supplier Material materials with Flexural yield strength of 370 MPa | dry | ISO 178 | ||
120 °C | 150 MPa Show Supplier Material materials with Flexural yield strength of 150 MPa | dry | ISO 178 | |
160 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
180 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
200 °C | 65 MPa Show Supplier Material materials with Flexural yield strength of 65 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 12 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 15 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 15 kJ/m² | dry | ISO 179/1eA | |
23 °C | 25 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 25 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 100 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 315 MPa Show Supplier Material materials with Zugfestigkeit of 315 MPa | dry | ISO 527-1/-2 |
155 MPa Show Supplier Material materials with Zugfestigkeit of 155 MPa | conditioned | ISO 527-1/-2 | ||
235 MPa Show Supplier Material materials with Zugfestigkeit of 235 MPa | dry | ISO 527-1/-2 | ||
100 °C | 115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | dry | ISO 527-1/-2 | |
150 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |
160 °C | 80 MPa Show Supplier Material materials with Zugfestigkeit of 80 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 3e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperaturleitfähigkeit | 1.18e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.18e-07 mm²/s | dry | - | ||
Wärmeformbeständigkeitstemperatur | 210 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 210 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4 [-] | dry | IEC 60250 | 5GHz |
4.1 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.1 [-] | dry | IEC 60250 | 1GHz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | dry | IEC 62631-2-1 | 1MHz | |
4.9 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.9 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
5.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 5.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
12 [-] Show Supplier Material materials with Dielektrizitätskonstante of 12 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Kriechstromfestigkeit | 500 V Show Supplier Material materials with Kriechstromfestigkeit of 500 V | dry | IEC 60112 | |
Verlustfaktor | 116 [-] Show Supplier Material materials with Verlustfaktor of 116 [-] | dry | IEC 60250 | 5GHz |
127 [-] Show Supplier Material materials with Verlustfaktor of 127 [-] | dry | IEC 60250 | 1GHz | |
270 [-] Show Supplier Material materials with Verlustfaktor of 270 [-] | dry | IEC 62631-2-1 | 1MHz | |
360 [-] Show Supplier Material materials with Verlustfaktor of 360 [-] | dry | IEC 62631-2-1 | 100Hz | |
770 [-] Show Supplier Material materials with Verlustfaktor of 770 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3250 [-] Show Supplier Material materials with Verlustfaktor of 3250 [-] | conditioned | IEC 62631-2-1 | 100Hz |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Density of melt | 1360 g/cm³ Show Supplier Material materials with Density of melt of 1360 g/cm³ | dry | - | ||
Schmelzmassenflussrate | 275 °C | 40 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 40 g/10min | dry | ISO 1133 | |
Schrumpfung | 0.2 % Show Supplier Material materials with Schrumpfung of 0.2 % | dry | ISO 294-4 | Parallel | |
0.9 % Show Supplier Material materials with Schrumpfung of 0.9 % | dry | ISO 294-4 | Normal | ||
Specific heat capacity melt | 1870 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1870 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.3 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.3 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Pump Housings, Front End Modules, Engine mounts, Top Mounts, Torque Rods, Suspension System Top Mounts | |
Fillers | 50% Glass Fiber |