Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.29 g/cm³ Show Supplier Material materials with Dichte of 1.29 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.6 % Show Supplier Material materials with Moisture absorption of 2.6 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 2.65 % Show Supplier Material materials with Wasserabsorption of 2.65 % | dry | ISO 62 | at 23°C after 24h |
9.5 % Show Supplier Material materials with Wasserabsorption of 9.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 11 GPa Show Supplier Material materials with Biegemodul of 11 GPa | conditioned | ISO 178 | |
20 GPa Show Supplier Material materials with Biegemodul of 20 GPa | dry | ISO 178 | ||
120 °C | 10.5 GPa Show Supplier Material materials with Biegemodul of 10.5 GPa | dry | ISO 178 | |
160 °C | 10 GPa Show Supplier Material materials with Biegemodul of 10 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 1.7 % Show Supplier Material materials with Dehnung of 1.7 % | dry | ISO 527-1/-2 |
1.7 % Show Supplier Material materials with Dehnung of 1.7 % | dry | ISO 527-1/-2 | ||
3 % Show Supplier Material materials with Dehnung of 3 % | conditioned | ISO 527-1/-2 | ||
120 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 | |
160 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 | |
180 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 | |
200 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 23.5 GPa Show Supplier Material materials with Elastizitätsmodul of 23.5 GPa | dry | ISO 527-1/-2 |
13.5 GPa Show Supplier Material materials with Elastizitätsmodul of 13.5 GPa | conditioned | ISO 527-1/-2 | ||
23.5 GPa Show Supplier Material materials with Elastizitätsmodul of 23.5 GPa | dry | ISO 527-1/-2 | ||
120 °C | 11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | dry | ISO 527-1/-2 | |
160 °C | 10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | dry | ISO 527-1/-2 | |
180 °C | 9.5 GPa Show Supplier Material materials with Elastizitätsmodul of 9.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 8.7 GPa Show Supplier Material materials with Elastizitätsmodul of 8.7 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 220 MPa Show Supplier Material materials with Flexural yield strength of 220 MPa | conditioned | ISO 178 | |
360 MPa Show Supplier Material materials with Flexural yield strength of 360 MPa | dry | ISO 178 | ||
120 °C | 195 MPa Show Supplier Material materials with Flexural yield strength of 195 MPa | dry | ISO 178 | |
160 °C | 160 MPa Show Supplier Material materials with Flexural yield strength of 160 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 6.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 6.5 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | dry | ISO 179/1eA | |
23 °C | 14.0 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 14.0 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 60 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 60 kJ/m² | dry | ISO 179/1eU | |
23 °C | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 320 MPa Show Supplier Material materials with Zugfestigkeit of 320 MPa | dry | ISO 527-1/-2 |
165 MPa Show Supplier Material materials with Zugfestigkeit of 165 MPa | conditioned | ISO 527-1/-2 | ||
250 MPa Show Supplier Material materials with Zugfestigkeit of 250 MPa | dry | ISO 527-1/-2 | ||
120 °C | 135 MPa Show Supplier Material materials with Zugfestigkeit of 135 MPa | dry | ISO 527-1/-2 | |
160 °C | 115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | dry | ISO 527-1/-2 | |
180 °C | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | dry | ISO 527-1/-2 | |
200 °C | 90 MPa Show Supplier Material materials with Zugfestigkeit of 90 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 8e-08 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 8e-08 1/K | dry | ISO 11359-1/-2 | Parallel | |
3.4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3.4e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 290 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 290 °C | dry | ISO 75-1/-2 | 2 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Volume resistivity | 10000 Ω·cm Show Supplier Material materials with Volume resistivity of 10000 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Automotive Bearing Cages, Crankshaft Balance Gears, Gears | |
Fillers | 30% Carbon Fiber |