Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.2 g/cm³ Show Supplier Material materials with Dichte of 1.2 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2 % Show Supplier Material materials with Moisture absorption of 2 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6.8 % Show Supplier Material materials with Wasserabsorption of 6.8 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 2.6 GPa Show Supplier Material materials with Biegemodul of 2.6 GPa | conditioned | ISO 178 | |
5.2 GPa Show Supplier Material materials with Biegemodul of 5.2 GPa | dry | ISO 178 | ||
120 °C | 1.7 GPa Show Supplier Material materials with Biegemodul of 1.7 GPa | dry | ISO 178 | |
160 °C | 1.5 GPa Show Supplier Material materials with Biegemodul of 1.5 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 5 % Show Supplier Material materials with Dehnung of 5 % | dry | ISO 527-1/-2 |
5 % Show Supplier Material materials with Dehnung of 5 % | dry | ISO 527-1/-2 | ||
15 % Show Supplier Material materials with Dehnung of 15 % | conditioned | ISO 527-1/-2 | ||
120 °C | 22 % Show Supplier Material materials with Dehnung of 22 % | dry | ISO 527-1/-2 | |
160 °C | 25 % Show Supplier Material materials with Dehnung of 25 % | dry | ISO 527-1/-2 | |
180 °C | 26 % Show Supplier Material materials with Dehnung of 26 % | dry | ISO 527-1/-2 | |
200 °C | 27 % Show Supplier Material materials with Dehnung of 27 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 6 GPa Show Supplier Material materials with Elastizitätsmodul of 6 GPa | dry | ISO 527-1/-2 |
3 GPa Show Supplier Material materials with Elastizitätsmodul of 3 GPa | conditioned | ISO 527-1/-2 | ||
5.5 GPa Show Supplier Material materials with Elastizitätsmodul of 5.5 GPa | dry | ISO 527-1/-2 | ||
40 °C | 5.1 GPa Show Supplier Material materials with Elastizitätsmodul of 5.1 GPa | dry | ISO 527-1/-2 | |
120 °C | 1.7 GPa Show Supplier Material materials with Elastizitätsmodul of 1.7 GPa | dry | ISO 527-1/-2 | |
160 °C | 1.4 GPa Show Supplier Material materials with Elastizitätsmodul of 1.4 GPa | dry | ISO 527-1/-2 | |
180 °C | 1.2 GPa Show Supplier Material materials with Elastizitätsmodul of 1.2 GPa | dry | ISO 527-1/-2 | |
200 °C | 1.1 GPa Show Supplier Material materials with Elastizitätsmodul of 1.1 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 85 MPa Show Supplier Material materials with Flexural yield strength of 85 MPa | conditioned | ISO 178 | |
180 MPa Show Supplier Material materials with Flexural yield strength of 180 MPa | dry | ISO 178 | ||
120 °C | 55.0 MPa Show Supplier Material materials with Flexural yield strength of 55.0 MPa | dry | ISO 178 | |
160 °C | 42 MPa Show Supplier Material materials with Flexural yield strength of 42 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 10 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 20 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 20 kJ/m² | dry | ISO 179/1eA | |
23 °C | 30 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 30 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 170 MPa Show Supplier Material materials with Zugfestigkeit of 170 MPa | dry | ISO 527-1/-2 |
60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | conditioned | ISO 527-1/-2 | ||
115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | dry | ISO 527-1/-2 | ||
120 °C | 51 MPa Show Supplier Material materials with Zugfestigkeit of 51 MPa | dry | ISO 527-1/-2 | |
160 °C | 44 MPa Show Supplier Material materials with Zugfestigkeit of 44 MPa | dry | ISO 527-1/-2 | |
180 °C | 38 MPa Show Supplier Material materials with Zugfestigkeit of 38 MPa | dry | ISO 527-1/-2 | |
200 °C | 31 MPa Show Supplier Material materials with Zugfestigkeit of 31 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 185 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 185 °C | dry | ISO 75-1/-2 | 2 MPa | |
210 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 210 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzvolumenflussrate | 275 °C | 40 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 40 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 0.25 % Show Supplier Material materials with Schrumpfung of 0.25 % | dry | ISO 294-4 | Parallel | |
1.2 % Show Supplier Material materials with Schrumpfung of 1.2 % | dry | ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Application areas | Clean Air Inlet Ducts, Hot Charged Air Ducts, Cold Charged Air Ducts | |
Fillers | 15% Glass Fiber |