Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.45 g/cm³ Show Supplier Material materials with Dichte of 1.45 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2 % Show Supplier Material materials with Moisture absorption of 2 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 0.4 % Show Supplier Material materials with Wasserabsorption of 0.4 % | dry | ISO 62 | at 23°C after 24h |
4.7 % Show Supplier Material materials with Wasserabsorption of 4.7 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 10.5 GPa Show Supplier Material materials with Biegemodul of 10.5 GPa | dry | ISO 178 | |
11 GPa Show Supplier Material materials with Biegemodul of 11 GPa | conditioned | ISO 178 | ||
120 °C | 9.9 GPa Show Supplier Material materials with Biegemodul of 9.9 GPa | dry | ISO 178 | |
160 °C | 5.8 GPa Show Supplier Material materials with Biegemodul of 5.8 GPa | dry | ISO 178 | |
180 °C | 4.6 GPa Show Supplier Material materials with Biegemodul of 4.6 GPa | dry | ISO 178 | |
200 °C | 4.2 GPa Show Supplier Material materials with Biegemodul of 4.2 GPa | dry | ISO 178 | |
210 °C | 4.1 GPa Show Supplier Material materials with Biegemodul of 4.1 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2.3 % Show Supplier Material materials with Dehnung of 2.3 % | dry | ISO 527-1/-2 |
2 % Show Supplier Material materials with Dehnung of 2 % | conditioned | ISO 527-1/-2 | ||
2.1 % Show Supplier Material materials with Dehnung of 2.1 % | dry | ISO 527-1/-2 | ||
40 °C | 1.9 % Show Supplier Material materials with Dehnung of 1.9 % | dry | ISO 527-1/-2 | |
40 °C | 2.2 % Show Supplier Material materials with Dehnung of 2.2 % | conditioned | ISO 527-1/-2 | |
80 °C | 1.9 % Show Supplier Material materials with Dehnung of 1.9 % | dry | ISO 527-1/-2 | |
80 °C | 2.8 % Show Supplier Material materials with Dehnung of 2.8 % | conditioned | ISO 527-1/-2 | |
100 °C | 2.0 % Show Supplier Material materials with Dehnung of 2.0 % | dry | ISO 527-1/-2 | |
100 °C | 5.2 % Show Supplier Material materials with Dehnung of 5.2 % | conditioned | ISO 527-1/-2 | |
120 °C | 2.1 % Show Supplier Material materials with Dehnung of 2.1 % | dry | ISO 527-1/-2 | |
150 °C | 3.5 % Show Supplier Material materials with Dehnung of 3.5 % | dry | ISO 527-1/-2 | |
160 °C | 4.5 % Show Supplier Material materials with Dehnung of 4.5 % | dry | ISO 527-1/-2 | |
180 °C | 5.7 % Show Supplier Material materials with Dehnung of 5.7 % | dry | ISO 527-1/-2 | |
200 °C | 6 % Show Supplier Material materials with Dehnung of 6 % | dry | ISO 527-1/-2 | |
210 °C | 0.006 % Show Supplier Material materials with Dehnung of 0.006 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 12 GPa Show Supplier Material materials with Elastizitätsmodul of 12 GPa | dry | ISO 527-1/-2 |
11.3 GPa Show Supplier Material materials with Elastizitätsmodul of 11.3 GPa | dry | ISO 527-1/-2 | ||
11.8 GPa Show Supplier Material materials with Elastizitätsmodul of 11.8 GPa | conditioned | ISO 527-1/-2 | ||
40 °C | 11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | dry, conditioned | ISO 527-1/-2 | |
80 °C | 10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | conditioned | ISO 527-1/-2 | |
80 °C | 10.5 GPa Show Supplier Material materials with Elastizitätsmodul of 10.5 GPa | dry | ISO 527-1/-2 | |
100 °C | 6.4 GPa Show Supplier Material materials with Elastizitätsmodul of 6.4 GPa | conditioned | ISO 527-1/-2 | |
100 °C | 10.3 GPa Show Supplier Material materials with Elastizitätsmodul of 10.3 GPa | dry | ISO 527-1/-2 | |
120 °C | 10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | dry | ISO 527-1/-2 | |
150 °C | 7.5 GPa Show Supplier Material materials with Elastizitätsmodul of 7.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 6.2 GPa Show Supplier Material materials with Elastizitätsmodul of 6.2 GPa | dry | ISO 527-1/-2 | |
180 °C | 5 GPa Show Supplier Material materials with Elastizitätsmodul of 5 GPa | dry | ISO 527-1/-2 | |
200 °C | 4.5 GPa Show Supplier Material materials with Elastizitätsmodul of 4.5 GPa | dry | ISO 527-1/-2 | |
210 °C | 4.3 GPa Show Supplier Material materials with Elastizitätsmodul of 4.3 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | conditioned | ISO 178 | |
270 MPa Show Supplier Material materials with Flexural yield strength of 270 MPa | dry | ISO 178 | ||
120 °C | 230 MPa Show Supplier Material materials with Flexural yield strength of 230 MPa | dry | ISO 178 | |
160 °C | 150 MPa Show Supplier Material materials with Flexural yield strength of 150 MPa | dry | ISO 178 | |
180 °C | 122 MPa Show Supplier Material materials with Flexural yield strength of 122 MPa | dry | ISO 178 | |
200 °C | 108 MPa Show Supplier Material materials with Flexural yield strength of 108 MPa | dry | ISO 178 | |
210 °C | 104 MPa Show Supplier Material materials with Flexural yield strength of 104 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 9 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | dry | ISO 179/1eA | |
23 °C | 9 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 9.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9.5 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 35 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 35 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 40 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | dry | ISO 179/1eU | |
23 °C | 40 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 45 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 45 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 220 MPa Show Supplier Material materials with Zugfestigkeit of 220 MPa | dry | ISO 527-1/-2 |
180 MPa Show Supplier Material materials with Zugfestigkeit of 180 MPa | conditioned | ISO 527-1/-2 | ||
190 MPa Show Supplier Material materials with Zugfestigkeit of 190 MPa | dry | ISO 527-1/-2 | ||
40 °C | 165 MPa Show Supplier Material materials with Zugfestigkeit of 165 MPa | dry | ISO 527-1/-2 | |
40 °C | 170 MPa Show Supplier Material materials with Zugfestigkeit of 170 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 130 MPa Show Supplier Material materials with Zugfestigkeit of 130 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 155 MPa Show Supplier Material materials with Zugfestigkeit of 155 MPa | dry | ISO 527-1/-2 | |
100 °C | 95 MPa Show Supplier Material materials with Zugfestigkeit of 95 MPa | conditioned | ISO 527-1/-2 | |
100 °C | 150 MPa Show Supplier Material materials with Zugfestigkeit of 150 MPa | dry | ISO 527-1/-2 | |
120 °C | 140 MPa Show Supplier Material materials with Zugfestigkeit of 140 MPa | dry | ISO 527-1/-2 | |
150 °C | 110 MPa Show Supplier Material materials with Zugfestigkeit of 110 MPa | dry | ISO 527-1/-2 | |
160 °C | 97 MPa Show Supplier Material materials with Zugfestigkeit of 97 MPa | dry | ISO 527-1/-2 | |
180 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |
200 °C | 75 MPa Show Supplier Material materials with Zugfestigkeit of 75 MPa | dry | ISO 527-1/-2 | |
210 °C | 71 MPa Show Supplier Material materials with Zugfestigkeit of 71 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 160 °C Show Supplier Material materials with Glasübergangstemperatur of 160 °C | dry | ASTM D5026/D7028 | DMTA (tan d) | |
Koeffizient der thermischen Ausdehnung | 1.8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.8e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
5.8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 5.8e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 335 °C Show Supplier Material materials with Schmelzpunkt of 335 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 317 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 317 °C | dry | ISO 75-1/-2 | 2 MPa | |
330 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 330 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Structural Parts with ForTii® Ace | |
Fillers | 30% Glass Fiber |