Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 21.36 g/cm³ Show Supplier Material materials with Dichte of 21.36 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 1200.0 °C | 52 % Show Supplier Material materials with Dehnung of 52 % | |
1400.0 °C | 48 % Show Supplier Material materials with Dehnung of 48 % | ||
Härte, Vickers | 23.0 °C | 73 [-] Show Supplier Material materials with Härte, Vickers of 73 [-] | |
Kriechfestigkeit | 1200.0 °C | 12 MPa Show Supplier Material materials with Kriechfestigkeit of 12 MPa | 10,000 h (extrapolated data) |
1400.0 °C | 4.3 MPa Show Supplier Material materials with Kriechfestigkeit of 4.3 MPa | 10,000 h (extrapolated data) | |
Streckgrenze Rp 0,2 | 1200.0 °C | 19 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 19 MPa | |
1400.0 °C | 15 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 15 MPa | ||
Zugfestigkeit | 1200.0 °C | 24 MPa Show Supplier Material materials with Zugfestigkeit of 24 MPa | |
1400.0 °C | 16 MPa Show Supplier Material materials with Zugfestigkeit of 16 MPa | ||
Thermisch
Property | Temperature | Value |
---|---|---|
Schmelzpunkt | 1769 °C Show Supplier Material materials with Schmelzpunkt of 1769 °C | |
Wärmeleitfähigkeit | 20.0 °C | 71.5 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 71.5 W/(m·K) |
1200.0 °C | 84.2 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 84.2 W/(m·K) | |
1400.0 °C | 85 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 85 W/(m·K) | |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 1.2E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1.2E-7 Ω·m |
1200.0 °C | 5.4E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 5.4E-7 Ω·m | |
1400.0 °C | 5.9E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 5.9E-7 Ω·m | |