Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 18.74 g/cm³ Show Supplier Material materials with Dichte of 18.74 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 43 % Show Supplier Material materials with Dehnung of 43 % | |
1200.0 °C | 29 % Show Supplier Material materials with Dehnung of 29 % | ||
1400.0 °C | 36 % Show Supplier Material materials with Dehnung of 36 % | ||
1600.0 °C | 34 % Show Supplier Material materials with Dehnung of 34 % | ||
Elastizitätsmodul | 20.0 °C | 246 GPa Show Supplier Material materials with Elastizitätsmodul of 246 GPa | |
1200.0 °C | 179 GPa Show Supplier Material materials with Elastizitätsmodul of 179 GPa | ||
1400.0 °C | 166 GPa Show Supplier Material materials with Elastizitätsmodul of 166 GPa | ||
1600.0 °C | 145 GPa Show Supplier Material materials with Elastizitätsmodul of 145 GPa | ||
Härte, Vickers | 23.0 °C | 99 [-] Show Supplier Material materials with Härte, Vickers of 99 [-] | |
Kriechfestigkeit | 1200.0 °C | 2.8 MPa Show Supplier Material materials with Kriechfestigkeit of 2.8 MPa | 10,000 h (extrapolated data) |
1400.0 °C | 2.2 MPa Show Supplier Material materials with Kriechfestigkeit of 2.2 MPa | 10,000 h (extrapolated data) | |
1600.0 °C | 0.8 MPa Show Supplier Material materials with Kriechfestigkeit of 0.8 MPa | 10,000 h (extrapolated data) | |
Norton Exponent | 1200.0 °C | 3.5 [-] Show Supplier Material materials with Norton Exponent of 3.5 [-] | |
1400.0 °C | 3.6 [-] Show Supplier Material materials with Norton Exponent of 3.6 [-] | ||
1600.0 °C | 3.5 [-] Show Supplier Material materials with Norton Exponent of 3.5 [-] | ||
Streckgrenze Rp 0,2 | 20.0 °C | 130 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 130 MPa | |
1200.0 °C | 58.6 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 58.6 MPa | ||
1400.0 °C | 35.7 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 35.7 MPa | ||
1600.0 °C | 24.4 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 24.4 MPa | ||
Zugfestigkeit | 20.0 °C | 377 MPa Show Supplier Material materials with Zugfestigkeit of 377 MPa | |
1200.0 °C | 92.7 MPa Show Supplier Material materials with Zugfestigkeit of 92.7 MPa | ||
1400.0 °C | 51.4 MPa Show Supplier Material materials with Zugfestigkeit of 51.4 MPa | ||
1600.0 °C | 27.4 MPa Show Supplier Material materials with Zugfestigkeit of 27.4 MPa | ||
Thermisch
Property | Temperature | Value |
---|---|---|
Schmelzpunkt | 1830 - 1855 °C Show Supplier Material materials with Schmelzpunkt of 1830 - 1855 °C | |
Wärmeleitfähigkeit | 20.0 °C | 34 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 34 W/(m·K) |
1200.0 °C | 60.7 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 60.7 W/(m·K) | |
1400.0 °C | 63.5 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 63.5 W/(m·K) | |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 2.1E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 2.1E-7 Ω·m |
1151.0 °C | 5.2E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 5.2E-7 Ω·m | |
1400.0 °C | 5.8E-7 Ω·m Show Supplier Material materials with spezifischer Widerstand of 5.8E-7 Ω·m | |