Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 18.7 g/cm³ Show Supplier Material materials with Dichte of 18.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 35.8 % Show Supplier Material materials with Dehnung of 35.8 % | |
Elastizitätsmodul | 20.0 °C | 247.8 GPa Show Supplier Material materials with Elastizitätsmodul of 247.8 GPa | |
1200.0 °C | 180 GPa Show Supplier Material materials with Elastizitätsmodul of 180 GPa | ||
1400.0 °C | 170 GPa Show Supplier Material materials with Elastizitätsmodul of 170 GPa | ||
1600.0 °C | 150 GPa Show Supplier Material materials with Elastizitätsmodul of 150 GPa | ||
Härte, Vickers | 23.0 °C | 130 [-] Show Supplier Material materials with Härte, Vickers of 130 [-] | |
Kriechfestigkeit | 1200.0 °C | 13.6 MPa Show Supplier Material materials with Kriechfestigkeit of 13.6 MPa | 10,000 h (extrapolated data) |
1400.0 °C | 7.1 MPa Show Supplier Material materials with Kriechfestigkeit of 7.1 MPa | 10,000 h (extrapolated data) | |
1600.0 °C | 6.1 MPa Show Supplier Material materials with Kriechfestigkeit of 6.1 MPa | 10,000 h (extrapolated data) | |
Norton Exponent | 1200.0 °C | 6.3 [-] Show Supplier Material materials with Norton Exponent of 6.3 [-] | |
1400.0 °C | 10 [-] Show Supplier Material materials with Norton Exponent of 10 [-] | ||
1600.0 °C | 9.3 [-] Show Supplier Material materials with Norton Exponent of 9.3 [-] | ||
Streckgrenze Rp 0,2 | 20.0 °C | 147.4 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 147.4 MPa | |
Zugfestigkeit | 23.0 °C | 464.7 MPa Show Supplier Material materials with Zugfestigkeit of 464.7 MPa |
Thermisch
Property | Value |
---|---|
Schmelzpunkt | 1830 - 1855 °C Show Supplier Material materials with Schmelzpunkt of 1830 - 1855 °C |