Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 17.3 % Show Material materials with Dehnung of 17.3 % | Predicted Value, A200 | ||||
18.4 % Show Material materials with Dehnung of 18.4 % | Predicted Value, A80 | |||||
20.3 % Show Material materials with Dehnung of 20.3 % | Predicted Value, A80 Transverse | |||||
21.1 % Show Material materials with Dehnung of 21.1 % | Predicted Value, A5 | |||||
21.4 % Show Material materials with Dehnung of 21.4 % | Predicted Value, Transverse | |||||
22.5 % Show Material materials with Dehnung of 22.5 % | Predicted Value, A50 | |||||
20 °C | 22 % Show Material materials with Dehnung of 22 % | thermomechanically rolled | EN 10028-5 | Flat | ||
Elastizitätsmodul | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel | ||||
Flächenreduzierung | 40.3 % Show Material materials with Flächenreduzierung of 40.3 % | Predicted Value | ||||
44.3 % Show Material materials with Flächenreduzierung of 44.3 % | Predicted Value, Transverse | |||||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Scherfestigkeit | 558.8 MPa Show Material materials with Scherfestigkeit of 558.8 MPa | Predicted Value | ||||
Schubmodule | 79.6 GPa Show Material materials with Schubmodule of 79.6 GPa | Predicted Value | ||||
Streckgrenze | 254.6 MPa Show Material materials with Streckgrenze of 254.6 MPa | Predicted Value, RP1 | ||||
318.5 MPa Show Material materials with Streckgrenze of 318.5 MPa | Predicted Value, RP1 Transverse | |||||
357.1 MPa Show Material materials with Streckgrenze of 357.1 MPa | Predicted Value, RP02 | |||||
393.4 MPa Show Material materials with Streckgrenze of 393.4 MPa | Predicted Value, Transverse | |||||
453.7 MPa Show Material materials with Streckgrenze of 453.7 MPa | Predicted Value, RP02 Transverse | |||||
468.2 MPa Show Material materials with Streckgrenze of 468.2 MPa | Predicted Value, RP05 | |||||
494.9 MPa Show Material materials with Streckgrenze of 494.9 MPa | Predicted Value, RP002 | |||||
20 °C | 345 MPa Show Material materials with Streckgrenze of 345 MPa | thermomechanically rolled | EN 10028-5 | Flat | ||
20 °C | 355 MPa Show Material materials with Streckgrenze of 355 MPa | thermomechanically rolled | EN 10028-5 | Flat | ||
Zugfestigkeit | 20 °C | 450 - 610 MPa Show Material materials with Zugfestigkeit of 450 - 610 MPa | thermomechanically rolled | EN 10028-5 | Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 11.74 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 11.74 1/K | Predicted Value |
Spezifische Wärmekapazität | 455 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 455 J/(kg·K) | Predicted Value |
Wärmeleitfähigkeit | 38.03 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.03 W/(m·K) | Predicted Value |
Elektrisch
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | thermomechanically rolled | EN 10028-5 | Flat |
Kohlenstoff | 0.14 % Show Material materials with Kohlenstoff of 0.14 % | thermomechanically rolled | EN 10028-5 | Flat |
Mangan | 1.6 % Show Material materials with Mangan of 1.6 % | thermomechanically rolled | EN 10028-5 | Flat |
Molybdän | 0.2 % Show Material materials with Molybdän of 0.2 % | thermomechanically rolled | EN 10028-5 | Flat |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % | thermomechanically rolled | EN 10028-5 | Flat |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | thermomechanically rolled | EN 10028-5 | Flat |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % | thermomechanically rolled | EN 10028-5 | Flat |
Schwefel | 0.008 % Show Material materials with Schwefel of 0.008 % | thermomechanically rolled | EN 10028-5 | Flat |
0.015 % Show Material materials with Schwefel of 0.015 % | thermomechanically rolled | EN 10028-5 | Flat | |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | thermomechanically rolled | EN 10028-5 | Flat |
Stickstoff | 0.015 % Show Material materials with Stickstoff of 0.015 % | thermomechanically rolled | EN 10028-5 | Flat |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | thermomechanically rolled | EN 10028-5 | Flat |
Vanadium | 0.1 % Show Material materials with Vanadium of 0.1 % | thermomechanically rolled | EN 10028-5 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |