General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 1.7 % Show Supplier Material materials with Absorción de agua of 1.7 % | dry | ISO 62 | at 23°C after 24h |
5.9 % Show Supplier Material materials with Absorción de agua of 5.9 % | dry | Sim. to ISO 62 | ||
Densidad | 1.67 g/cm³ Show Supplier Material materials with Densidad of 1.67 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | dry | Sim. to ISO 62 | |
Índice límite de óxigeno | 37 % Show Supplier Material materials with Índice límite de óxigeno of 37 % | dry | ISO 4589-1/-2 |
Mecánica
Property | Temperature | Value | Condition | Thickness | Testing Standard | Comment |
---|---|---|---|---|---|---|
Elongación | 2.4 % Show Supplier Material materials with Elongación of 2.4 % | dry | 1 mm | ISO 527-1/-2 | ||
2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | ||||
3.5 % Show Supplier Material materials with Elongación of 3.5 % | conditioned | ISO 527-1/-2 | ||||
3.8 % Show Supplier Material materials with Elongación of 3.8 % | conditioned | ISO 527-1/-2 | ||||
120 °C | 4 % Show Supplier Material materials with Elongación of 4 % | dry | ISO 527-1/-2 | |||
160 °C | 4 % Show Supplier Material materials with Elongación of 4 % | dry | ISO 527-1/-2 | |||
Flexural yield strength | 190 MPa Show Supplier Material materials with Flexural yield strength of 190 MPa | conditioned | ISO 178 | |||
260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | dry | ISO 178 | ||||
120 °C | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | dry | ISO 178 | |||
160 °C | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | dry | ISO 178 | |||
Módulo de flexión | 7.3 GPa Show Supplier Material materials with Módulo de flexión of 7.3 GPa | conditioned | ISO 178 | |||
11 GPa Show Supplier Material materials with Módulo de flexión of 11 GPa | dry | ISO 178 | ||||
120 °C | 6.5 GPa Show Supplier Material materials with Módulo de flexión of 6.5 GPa | dry | ISO 178 | |||
160 °C | 5 GPa Show Supplier Material materials with Módulo de flexión of 5 GPa | dry | ISO 178 | |||
Módulo elástico | 8 GPa Show Supplier Material materials with Módulo elástico of 8 GPa | conditioned | ISO 527-1/-2 | |||
8 GPa Show Supplier Material materials with Módulo elástico of 8 GPa | conditioned | ISO 527-1/-2 | ||||
12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | dry | ISO 527-1/-2 | ||||
12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | dry | 1 mm | ISO 527-1/-2 | |||
120 °C | 7.5 GPa Show Supplier Material materials with Módulo elástico of 7.5 GPa | dry | ISO 527-1/-2 | |||
160 °C | 6.2 GPa Show Supplier Material materials with Módulo elástico of 6.2 GPa | dry | ISO 527-1/-2 | |||
Resistencia a la tracción | 120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | conditioned | ISO 527-1/-2 | |||
120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | conditioned | ISO 527-1/-2 | at low thickness | |||
180 MPa Show Supplier Material materials with Resistencia a la tracción of 180 MPa | dry | ISO 527-1/-2 | ||||
180 MPa Show Supplier Material materials with Resistencia a la tracción of 180 MPa | dry | 1 mm | ISO 527-1/-2 | at low thickness | ||
120 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | dry | ISO 527-1/-2 | |||
160 °C | 95 MPa Show Supplier Material materials with Resistencia a la tracción of 95 MPa | dry | ISO 527-1/-2 | |||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | dry, conditioned | ISO 179/1eA | ||
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry, conditioned | ISO 179/1eA | |||
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 50 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | dry, conditioned | ISO 179/1eU | ||
23 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | dry, conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Ball pressure temperature | 270 °C Show Supplier Material materials with Ball pressure temperature of 270 °C | dry | IEC 60695-10-2 | |||
Coeficiente de dilatación térmica | 2.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
5.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 1.59e-07 mm²/s Show Supplier Material materials with Difusividad térmica of 1.59e-07 mm²/s | dry | - | |||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 825 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C | dry | IEC 60695-2-13 | 0.75 mm | ||
850 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 850 °C | dry | IEC 60695-2-13 | 3 mm | |||
Inflamabilidad | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 110 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 110 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 120 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 120 °C | dry | UL746B | 0.75 mm | ||
Temperatura de flexión bajo carga | 290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 295 °C Show Supplier Material materials with Temperatura de fusión of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperatura de reblandecimiento Vicat | 290 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 290 °C | dry | ISO 306 | 50°C/h 50N | ||
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.6 [-] Show Supplier Material materials with Constante dieléctrica of 3.6 [-] | dry | IEC 60250 | 1GHz |
3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | conditioned | IEC 60250 | 1GHz | |
4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 1MHz | |
4.3 [-] Show Supplier Material materials with Constante dieléctrica of 4.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
10 [-] Show Supplier Material materials with Constante dieléctrica of 10 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 60 [-] Show Supplier Material materials with Factor de disipación of 60 [-] | dry | IEC 62631-2-1 | 100Hz |
160 [-] Show Supplier Material materials with Factor de disipación of 160 [-] | dry | IEC 62631-2-1 | 1MHz | |
250 [-] Show Supplier Material materials with Factor de disipación of 250 [-] | dry | IEC 60250 | 1GHz | |
325 [-] Show Supplier Material materials with Factor de disipación of 325 [-] | conditioned | IEC 60250 | 1GHz | |
700 [-] Show Supplier Material materials with Factor de disipación of 700 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3300 [-] Show Supplier Material materials with Factor de disipación of 3300 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 20 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 20 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+08 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+08 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 225 V Show Supplier Material materials with Índice de seguimiento comparativo of 225 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.4 % Show Supplier Material materials with Contracción of 0.4 % | dry | Sim. to ISO 294-4 | Parallel |
1.1 % Show Supplier Material materials with Contracción of 1.1 % | dry | Sim. to ISO 294-4 | Normal | |
Density of melt | 1470 g/cm³ Show Supplier Material materials with Density of melt of 1470 g/cm³ | dry | - | |
Specific heat capacity melt | 1480 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1480 J/(kg·K) | dry | - | |
Spiral flow length | 105 | dry | - | 1.0 mm 800 bar |
115 | dry | - | 1.0 mm 900 bar | |
125 | dry | - | 1.0 mm 1000 bar | |
36 | dry | - | 0.5mm 1200 bar | |
50 | dry | - | 0.5mm 1600 bar | |
74 | dry | - | 0.5mm 2000 bar | |
Thermal conductivity of melt | 0.344 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.344 W/(m·K) | dry | - | |
Viscosity number | 145 cm³/gr Show Supplier Material materials with Viscosity number of 145 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Firefighter helmets, Miniature Circuit Breakers, Reflow connectors, FPC connectors, WtB and BtB Connectors, Battery Connectors, Thermostatic Controls, Hair Curler Brushes, Automotive Connectors, Endlaminates (electro motors), Brushholders (electro motors), Coil insulation, Automotive e-motor Bobbins, Molded case circuit breakers, Motor Starter/Overload Relays, Endlaminates (electrical components), Brushholders (electrical components), Bobbins, Reflow connectors (3) | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |