General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 2.3 % Show Supplier Material materials with Absorción de agua of 2.3 % | dry | ISO 62 | at 23°C after 24h |
6.7 % Show Supplier Material materials with Absorción de agua of 6.7 % | dry | Sim. to ISO 62 | ||
Densidad | 1.48 g/cm³ Show Supplier Material materials with Densidad of 1.48 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.2 % Show Supplier Material materials with Moisture absorption of 2.2 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 | |
8 % Show Supplier Material materials with Elongación of 8 % | conditioned | ISO 527-1/-2 | ||
120 °C | 10 % Show Supplier Material materials with Elongación of 10 % | dry | ISO 527-1/-2 | |
160 °C | 11 % Show Supplier Material materials with Elongación of 11 % | dry | ISO 527-1/-2 | |
180 °C | 12 % Show Supplier Material materials with Elongación of 12 % | dry | ISO 527-1/-2 | |
200 °C | 12.5 % Show Supplier Material materials with Elongación of 12.5 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 330 MPa Show Supplier Material materials with Flexural yield strength of 330 MPa | dry | ISO 178 | |
120 °C | 115 MPa Show Supplier Material materials with Flexural yield strength of 115 MPa | dry | ISO 178 | |
160 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
180 °C | 90 MPa Show Supplier Material materials with Flexural yield strength of 90 MPa | dry | ISO 178 | |
200 °C | 75 MPa Show Supplier Material materials with Flexural yield strength of 75 MPa | dry | ISO 178 | |
Módulo de flexión | 7 GPa Show Supplier Material materials with Módulo de flexión of 7 GPa | conditioned | ISO 178 | |
13 GPa Show Supplier Material materials with Módulo de flexión of 13 GPa | dry | ISO 178 | ||
120 °C | 5 GPa Show Supplier Material materials with Módulo de flexión of 5 GPa | dry | ISO 178 | |
160 °C | 4.6 GPa Show Supplier Material materials with Módulo de flexión of 4.6 GPa | dry | ISO 178 | |
180 °C | 4.2 GPa Show Supplier Material materials with Módulo de flexión of 4.2 GPa | dry | ISO 178 | |
200 °C | 3.4 GPa Show Supplier Material materials with Módulo de flexión of 3.4 GPa | dry | ISO 178 | |
Módulo elástico | 7 GPa Show Supplier Material materials with Módulo elástico of 7 GPa | conditioned | ISO 527-1/-2 | |
13 GPa Show Supplier Material materials with Módulo elástico of 13 GPa | dry | ISO 527-1/-2 | ||
120 °C | 5 GPa Show Supplier Material materials with Módulo elástico of 5 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.6 GPa Show Supplier Material materials with Módulo elástico of 4.6 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.2 GPa Show Supplier Material materials with Módulo elástico of 4.2 GPa | dry | ISO 527-1/-2 | |
200 °C | 3.4 GPa Show Supplier Material materials with Módulo elástico of 3.4 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 125 MPa Show Supplier Material materials with Resistencia a la tracción of 125 MPa | conditioned | ISO 527-1/-2 | |
210 MPa Show Supplier Material materials with Resistencia a la tracción of 210 MPa | dry | ISO 527-1/-2 | ||
120 °C | 100 MPa Show Supplier Material materials with Resistencia a la tracción of 100 MPa | dry | ISO 527-1/-2 | |
160 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
180 °C | 75 MPa Show Supplier Material materials with Resistencia a la tracción of 75 MPa | dry | ISO 527-1/-2 | |
200 °C | 60 MPa Show Supplier Material materials with Resistencia a la tracción of 60 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 15 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 15 kJ/m² | dry | ISO 179/1eA | |
23 °C | 25 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 25 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | dry | ISO 179/1eU |
-30 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 105 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 105 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Difusividad térmica | 1.12e-07 mm²/s Show Supplier Material materials with Difusividad térmica of 1.12e-07 mm²/s | dry | - | ||
Temperatura de flexión bajo carga | 256 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 256 °C | dry | ISO 75-1/-2 | 2 MPa | |
270 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 270 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 282 °C Show Supplier Material materials with Temperatura de fusión of 282 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | 70 °C Show Supplier Material materials with Temperatura de transición del vidrio of 70 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Índice de seguimiento comparativo | 300 V Show Supplier Material materials with Índice de seguimiento comparativo of 300 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | dry | ISO 294-4 | Parallel |
1 % Show Supplier Material materials with Contracción of 1 % | dry | ISO 294-4 | Normal | |
Density of melt | 1320 g/cm³ Show Supplier Material materials with Density of melt of 1320 g/cm³ | dry | - | |
Specific heat capacity melt | 2130 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2130 J/(kg·K) | dry | - | |
Spiral flow length | 90 | dry | - | 1.0 mm 800 bar |
100 | dry | - | 1.0 mm 900 bar | |
110 | dry | - | 1.0 mm 1000 bar | |
Thermal conductivity of melt | 0.314 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.314 W/(m·K) | dry | - | |
Viscosity number | 155 cm³/gr Show Supplier Material materials with Viscosity number of 155 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Integrated Air Inlet Manifolds (up to 230°C), Hot Charged Air Ducts, Charge Air Cooler Caps | |
Fillers | 40% Glass Fiber |