Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 6.3 % Show Supplier Material materials with Absorción de agua of 6.3 % | dry | Sim. to ISO 62 |
Densidad | 1.35 g/cm³ Show Supplier Material materials with Densidad of 1.35 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.9 % Show Supplier Material materials with Moisture absorption of 1.9 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 |
3.6 % Show Supplier Material materials with Elongación of 3.6 % | dry | ISO 527-1/-2 | ||
7 % Show Supplier Material materials with Elongación of 7 % | conditioned | ISO 527-1/-2 | ||
120 °C | 10.8 % Show Supplier Material materials with Elongación of 10.8 % | dry | ISO 527-1/-2 | |
150 °C | 11.6 % Show Supplier Material materials with Elongación of 11.6 % | dry | ISO 527-1/-2 | |
160 °C | 11.8 % Show Supplier Material materials with Elongación of 11.8 % | dry | ISO 527-1/-2 | |
180 °C | 12.3 % Show Supplier Material materials with Elongación of 12.3 % | dry | ISO 527-1/-2 | |
200 °C | 12.8 % Show Supplier Material materials with Elongación of 12.8 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 165 MPa Show Supplier Material materials with Flexural yield strength of 165 MPa | conditioned | ISO 178 | |
290 MPa Show Supplier Material materials with Flexural yield strength of 290 MPa | dry | ISO 178 | ||
120 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
160 °C | 95 MPa Show Supplier Material materials with Flexural yield strength of 95 MPa | dry | ISO 178 | |
Módulo de flexión | 5.3 GPa Show Supplier Material materials with Módulo de flexión of 5.3 GPa | conditioned | ISO 178 | |
9.2 GPa Show Supplier Material materials with Módulo de flexión of 9.2 GPa | dry | ISO 178 | ||
120 °C | 4.2 GPa Show Supplier Material materials with Módulo de flexión of 4.2 GPa | dry | ISO 178 | |
160 °C | 3.7 GPa Show Supplier Material materials with Módulo de flexión of 3.7 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 10.4 GPa Show Supplier Material materials with Módulo elástico of 10.4 GPa | dry | ISO 527-1/-2 |
6 GPa Show Supplier Material materials with Módulo elástico of 6 GPa | conditioned | ISO 527-1/-2 | ||
9.8 GPa Show Supplier Material materials with Módulo elástico of 9.8 GPa | dry | ISO 527-1/-2 | ||
100 °C | 4.3 GPa Show Supplier Material materials with Módulo elástico of 4.3 GPa | dry | ISO 527-1/-2 | |
120 °C | 4.0 GPa Show Supplier Material materials with Módulo elástico of 4.0 GPa | dry | ISO 527-1/-2 | |
150 °C | 3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.4 GPa Show Supplier Material materials with Módulo elástico of 3.4 GPa | dry | ISO 527-1/-2 | |
180 °C | 3 GPa Show Supplier Material materials with Módulo elástico of 3 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.5 GPa Show Supplier Material materials with Módulo elástico of 2.5 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 235 MPa Show Supplier Material materials with Resistencia a la tracción of 235 MPa | dry | ISO 527-1/-2 |
110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | conditioned | ISO 527-1/-2 | ||
195 MPa Show Supplier Material materials with Resistencia a la tracción of 195 MPa | dry | ISO 527-1/-2 | ||
100 °C | 95 MPa Show Supplier Material materials with Resistencia a la tracción of 95 MPa | dry | ISO 527-1/-2 | |
120 °C | 90 MPa Show Supplier Material materials with Resistencia a la tracción of 90 MPa | dry | ISO 527-1/-2 | |
150 °C | 75 MPa Show Supplier Material materials with Resistencia a la tracción of 75 MPa | dry | ISO 527-1/-2 | |
160 °C | 70 MPa Show Supplier Material materials with Resistencia a la tracción of 70 MPa | dry | ISO 527-1/-2 | |
180 °C | 60 MPa Show Supplier Material materials with Resistencia a la tracción of 60 MPa | dry | ISO 527-1/-2 | |
200 °C | 47 MPa Show Supplier Material materials with Resistencia a la tracción of 47 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
23 °C | 25 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 25 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 110 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 110 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
7e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Difusividad térmica | 1.12e-07 mm²/s Show Supplier Material materials with Difusividad térmica of 1.12e-07 mm²/s | dry | - | ||
Temperatura de flexión bajo carga | 210 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 210 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.3 [-] Show Supplier Material materials with Constante dieléctrica of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Constante dieléctrica of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
5 [-] Show Supplier Material materials with Constante dieléctrica of 5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
20 [-] Show Supplier Material materials with Constante dieléctrica of 20 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 50 [-] Show Supplier Material materials with Factor de disipación of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Factor de disipación of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Factor de disipación of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Factor de disipación of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 25 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 25 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 500 V Show Supplier Material materials with Índice de seguimiento comparativo of 500 V | conditioned | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | dry | ISO 294-4 | Parallel |
1.1 % Show Supplier Material materials with Contracción of 1.1 % | dry | ISO 294-4 | Normal | |
Density of melt | 1150 g/cm³ Show Supplier Material materials with Density of melt of 1150 g/cm³ | dry | - | |
Specific heat capacity melt | 2110 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2110 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.27 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.27 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Fillers | 30% Glass Fiber |