General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 1.7 % Show Supplier Material materials with Absorción de agua of 1.7 % | dry | ISO 62 | at 23°C after 24h |
6.3 % Show Supplier Material materials with Absorción de agua of 6.3 % | dry | Sim. to ISO 62 | ||
Densidad | 1.49 g/cm³ Show Supplier Material materials with Densidad of 1.49 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.1 % Show Supplier Material materials with Moisture absorption of 2.1 % | dry | Sim. to ISO 62 | |
Índice límite de óxigeno | 48 % Show Supplier Material materials with Índice límite de óxigeno of 48 % | dry | ISO 4589-1/-2 |
Mecánica
Property | Temperature | Value | Condition | Thickness | Testing Standard | Comment |
---|---|---|---|---|---|---|
Elongación | 2.1 % Show Supplier Material materials with Elongación of 2.1 % | dry | 1 mm | ISO 527-1/-2 | ||
2.4 % Show Supplier Material materials with Elongación of 2.4 % | dry | 1 mm | ISO 527-1/-2 | |||
3.1 % Show Supplier Material materials with Elongación of 3.1 % | conditioned | ISO 527-1/-2 | ||||
Flexural yield strength | 200 MPa Show Supplier Material materials with Flexural yield strength of 200 MPa | conditioned | ISO 178 | |||
210 MPa Show Supplier Material materials with Flexural yield strength of 210 MPa | dry | ISO 178 | ||||
Módulo de flexión | 8 GPa Show Supplier Material materials with Módulo de flexión of 8 GPa | conditioned | ISO 178 | |||
10.5 GPa Show Supplier Material materials with Módulo de flexión of 10.5 GPa | dry | ISO 178 | ||||
Módulo elástico | 8.4 GPa Show Supplier Material materials with Módulo elástico of 8.4 GPa | conditioned | ISO 527-1/-2 | |||
11.8 GPa Show Supplier Material materials with Módulo elástico of 11.8 GPa | dry | 1 mm | ISO 527-1/-2 | |||
12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | dry | 1 mm | ISO 527-1/-2 | |||
Resistencia a la tracción | 100 MPa Show Supplier Material materials with Resistencia a la tracción of 100 MPa | conditioned | ISO 527-1/-2 | |||
140 MPa Show Supplier Material materials with Resistencia a la tracción of 140 MPa | dry | 1 mm | ISO 527-1/-2 | |||
160 MPa Show Supplier Material materials with Resistencia a la tracción of 160 MPa | dry | 1 mm | ISO 527-1/-2 | at low thickness | ||
Resistencia al choque, ensayo Charpy entallado | 23 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | conditioned | ISO 179/1eA | |||
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 50 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | dry | ISO 179/1eU | ||
23 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.7e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.7e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
7e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.8 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | |||
Glow Wire Ignition Temperature | 800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | dry | IEC 60695-2-13 | 0.8 mm | ||
800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | dry | IEC 60695-2-13 | 3 mm | |||
Inflamabilidad | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
V-0 | dry | IEC 60695-11-10 | 0.18 mm | UL recognition :Yes | ||
Relative temperature index, electrical | 120 °C Show Supplier Material materials with Relative temperature index, electrical of 120 °C | dry | UL746B | 0.18 mm | ||
Relative temperature index, mechanical impact | 115 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 115 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical strength | 115 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 115 °C | dry | UL746B | 0.4 mm | ||
Temperatura de flexión bajo carga | 285 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 285 °C | dry | ISO 75-1/-2 | 2 MPa | ||
Temperatura de fusión | 295 °C Show Supplier Material materials with Temperatura de fusión of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.8 [-] Show Supplier Material materials with Constante dieléctrica of 3.8 [-] | dry | IEC 60250 | 10GHz |
3.9 [-] Show Supplier Material materials with Constante dieléctrica of 3.9 [-] | dry | IEC 60250 | 1GHz | |
4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | conditioned | IEC 60250 | 10GHz | |
4.1 [-] Show Supplier Material materials with Constante dieléctrica of 4.1 [-] | dry | IEC 62631-2-1 | 1MHz | |
4.1 [-] Show Supplier Material materials with Constante dieléctrica of 4.1 [-] | conditioned | IEC 60250 | 1GHz | |
4.4 [-] Show Supplier Material materials with Constante dieléctrica of 4.4 [-] | dry | IEC 62631-2-1 | 100Hz | |
5 [-] Show Supplier Material materials with Constante dieléctrica of 5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
11 [-] Show Supplier Material materials with Constante dieléctrica of 11 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 72 [-] Show Supplier Material materials with Factor de disipación of 72 [-] | dry | IEC 62631-2-1 | 100Hz |
100 [-] Show Supplier Material materials with Factor de disipación of 100 [-] | dry | IEC 60250 | 10GHz | |
120 [-] Show Supplier Material materials with Factor de disipación of 120 [-] | dry | IEC 60250 | 1GHz | |
160 [-] Show Supplier Material materials with Factor de disipación of 160 [-] | conditioned | IEC 60250 | 10GHz | |
165 [-] Show Supplier Material materials with Factor de disipación of 165 [-] | dry | IEC 62631-2-1 | 1MHz | |
190 [-] Show Supplier Material materials with Factor de disipación of 190 [-] | conditioned | IEC 60250 | 1GHz | |
1000 [-] Show Supplier Material materials with Factor de disipación of 1000 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
2100 [-] Show Supplier Material materials with Factor de disipación of 2100 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 24 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 24 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 550 V Show Supplier Material materials with Índice de seguimiento comparativo of 550 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | USB-C Connectors, Miniature Circuit Breakers, DDR DIMM Connectors, Audio Jack Connectors, Molded case circuit breakers, Reflow connectors (2) | |
Certifications | Yellow Card Available | |
Fillers | 35% Glass Fiber |