Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 0.45 % Show Supplier Material materials with Absorción de agua of 0.45 % | dry | Sim. to ISO 62 |
Densidad | 1.66 g/cm³ Show Supplier Material materials with Densidad of 1.66 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.18 % Show Supplier Material materials with Moisture absorption of 0.18 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | |
Módulo elástico | 13 GPa Show Supplier Material materials with Módulo elástico of 13 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 185 MPa Show Supplier Material materials with Resistencia a la tracción of 185 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 8 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | dry | ISO 179/1eA |
23 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | dry | ISO 179/1eU |
23 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
4e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 4e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Difusividad térmica | 8.67e-08 mm²/s Show Supplier Material materials with Difusividad térmica of 8.67e-08 mm²/s | dry | - | ||
Temperatura de flexión bajo carga | 225 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 225 °C | dry | ISO 75-1/-2 | 2 MPa | |
250 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 250 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 255 °C Show Supplier Material materials with Temperatura de fusión of 255 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 3.5 [-] Show Supplier Material materials with Constante dieléctrica of 3.5 [-] | dry | IEC 62631-2-1 | 1MHz |
3.7 [-] Show Supplier Material materials with Constante dieléctrica of 3.7 [-] | dry | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 30 [-] Show Supplier Material materials with Factor de disipación of 30 [-] | dry | IEC 62631-2-1 | 100Hz |
130 [-] Show Supplier Material materials with Factor de disipación of 130 [-] | dry | IEC 62631-2-1 | 1MHz | |
Rigidez dieléctrica | 33 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 33 kV/mm | dry | IEC 60243-1 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 250 V Show Supplier Material materials with Índice de seguimiento comparativo of 250 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | dry | Sim. to ISO 294-4 | Parallel |
1 % Show Supplier Material materials with Contracción of 1 % | dry | Sim. to ISO 294-4 | Normal | |
Density of melt | 1350 g/cm³ Show Supplier Material materials with Density of melt of 1350 g/cm³ | dry | - | |
Specific heat capacity melt | 1670 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1670 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.195 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.195 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Bezels and AFL Frames, Foglamps, Lens holder Sun load, LED module frame | |
Certifications | Yellow Card Available | |
Fillers | 35% Glass Fiber |