General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 0.24 % Show Supplier Material materials with Absorción de agua of 0.24 % | dry | ISO 62 | at 23°C after 24h |
3.3 % Show Supplier Material materials with Absorción de agua of 3.3 % | dry | Sim. to ISO 62 | ||
Densidad | 1.66 g/cm³ Show Supplier Material materials with Densidad of 1.66 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 2.3 % Show Supplier Material materials with Elongación of 2.3 % | dry | ISO 527-1/-2 |
2 % Show Supplier Material materials with Elongación of 2 % | conditioned | ISO 527-1/-2 | ||
2.1 % Show Supplier Material materials with Elongación of 2.1 % | dry | ISO 527-1/-2 | ||
40 °C | 2 % Show Supplier Material materials with Elongación of 2 % | dry, conditioned | ISO 527-1/-2 | |
80 °C | 2 % Show Supplier Material materials with Elongación of 2 % | dry | ISO 527-1/-2 | |
80 °C | 2.6 % Show Supplier Material materials with Elongación of 2.6 % | conditioned | ISO 527-1/-2 | |
100 °C | 2.0 % Show Supplier Material materials with Elongación of 2.0 % | dry | ISO 527-1/-2 | |
100 °C | 3.4 % Show Supplier Material materials with Elongación of 3.4 % | conditioned | ISO 527-1/-2 | |
120 °C | 2.1 % Show Supplier Material materials with Elongación of 2.1 % | dry | ISO 527-1/-2 | |
150 °C | 3.4 % Show Supplier Material materials with Elongación of 3.4 % | dry | ISO 527-1/-2 | |
160 °C | 4.1 % Show Supplier Material materials with Elongación of 4.1 % | dry | ISO 527-1/-2 | |
180 °C | 4.9 % Show Supplier Material materials with Elongación of 4.9 % | dry | ISO 527-1/-2 | |
200 °C | 5 % Show Supplier Material materials with Elongación of 5 % | dry | ISO 527-1/-2 | |
210 °C | 0.005 % Show Supplier Material materials with Elongación of 0.005 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 360 MPa Show Supplier Material materials with Flexural yield strength of 360 MPa | conditioned | ISO 178 | |
380 MPa Show Supplier Material materials with Flexural yield strength of 380 MPa | dry | ISO 178 | ||
120 °C | 270 MPa Show Supplier Material materials with Flexural yield strength of 270 MPa | dry | ISO 178 | |
160 °C | 165 MPa Show Supplier Material materials with Flexural yield strength of 165 MPa | dry | ISO 178 | |
180 °C | 135 MPa Show Supplier Material materials with Flexural yield strength of 135 MPa | dry | ISO 178 | |
200 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
210 °C | 115 MPa Show Supplier Material materials with Flexural yield strength of 115 MPa | dry | ISO 178 | |
Módulo de flexión | 17 GPa Show Supplier Material materials with Módulo de flexión of 17 GPa | dry | ISO 178 | |
17.8 GPa Show Supplier Material materials with Módulo de flexión of 17.8 GPa | conditioned | ISO 178 | ||
120 °C | 15.7 GPa Show Supplier Material materials with Módulo de flexión of 15.7 GPa | dry | ISO 178 | |
160 °C | 10 GPa Show Supplier Material materials with Módulo de flexión of 10 GPa | dry | ISO 178 | |
180 °C | 8 GPa Show Supplier Material materials with Módulo de flexión of 8 GPa | dry | ISO 178 | |
200 °C | 7.4 GPa Show Supplier Material materials with Módulo de flexión of 7.4 GPa | dry | ISO 178 | |
210 °C | 7 GPa Show Supplier Material materials with Módulo de flexión of 7 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 18.5 GPa Show Supplier Material materials with Módulo elástico of 18.5 GPa | dry | ISO 527-1/-2 |
18 GPa Show Supplier Material materials with Módulo elástico of 18 GPa | dry | ISO 527-1/-2 | ||
18.9 GPa Show Supplier Material materials with Módulo elástico of 18.9 GPa | conditioned | ISO 527-1/-2 | ||
40 °C | 17.5 GPa Show Supplier Material materials with Módulo elástico of 17.5 GPa | dry, conditioned | ISO 527-1/-2 | |
80 °C | 16 GPa Show Supplier Material materials with Módulo elástico of 16 GPa | conditioned | ISO 527-1/-2 | |
80 °C | 17.3 GPa Show Supplier Material materials with Módulo elástico of 17.3 GPa | dry | ISO 527-1/-2 | |
100 °C | 11 GPa Show Supplier Material materials with Módulo elástico of 11 GPa | conditioned | ISO 527-1/-2 | |
100 °C | 17 GPa Show Supplier Material materials with Módulo elástico of 17 GPa | dry | ISO 527-1/-2 | |
120 °C | 16 GPa Show Supplier Material materials with Módulo elástico of 16 GPa | dry | ISO 527-1/-2 | |
150 °C | 11.5 GPa Show Supplier Material materials with Módulo elástico of 11.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 10 GPa Show Supplier Material materials with Módulo elástico of 10 GPa | dry | ISO 527-1/-2 | |
180 °C | 8 GPa Show Supplier Material materials with Módulo elástico of 8 GPa | dry | ISO 527-1/-2 | |
200 °C | 7.2 GPa Show Supplier Material materials with Módulo elástico of 7.2 GPa | dry | ISO 527-1/-2 | |
210 °C | 6.9 GPa Show Supplier Material materials with Módulo elástico of 6.9 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 300 MPa Show Supplier Material materials with Resistencia a la tracción of 300 MPa | dry | ISO 527-1/-2 |
250 MPa Show Supplier Material materials with Resistencia a la tracción of 250 MPa | conditioned | ISO 527-1/-2 | ||
260 MPa Show Supplier Material materials with Resistencia a la tracción of 260 MPa | dry | ISO 527-1/-2 | ||
40 °C | 220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | conditioned | ISO 527-1/-2 | |
40 °C | 235 MPa Show Supplier Material materials with Resistencia a la tracción of 235 MPa | dry | ISO 527-1/-2 | |
80 °C | 160 MPa Show Supplier Material materials with Resistencia a la tracción of 160 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 205 MPa Show Supplier Material materials with Resistencia a la tracción of 205 MPa | dry | ISO 527-1/-2 | |
100 °C | 125 MPa Show Supplier Material materials with Resistencia a la tracción of 125 MPa | conditioned | ISO 527-1/-2 | |
100 °C | 190 MPa Show Supplier Material materials with Resistencia a la tracción of 190 MPa | dry | ISO 527-1/-2 | |
120 °C | 170 MPa Show Supplier Material materials with Resistencia a la tracción of 170 MPa | dry | ISO 527-1/-2 | |
150 °C | 130 MPa Show Supplier Material materials with Resistencia a la tracción of 130 MPa | dry | ISO 527-1/-2 | |
160 °C | 120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | dry | ISO 527-1/-2 | |
180 °C | 100 MPa Show Supplier Material materials with Resistencia a la tracción of 100 MPa | dry | ISO 527-1/-2 | |
200 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
210 °C | 80 MPa Show Supplier Material materials with Resistencia a la tracción of 80 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 70 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 70 kJ/m² | dry | ISO 179/1eU | |
23 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 80 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 1.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperatura de flexión bajo carga | 320 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 320 °C | dry | ISO 75-1/-2 | 2 MPa | |
330 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 330 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 335 °C Show Supplier Material materials with Temperatura de fusión of 335 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | 160 °C Show Supplier Material materials with Temperatura de transición del vidrio of 160 °C | dry | ASTM D5026/D7028 | DMTA (tan d) |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Structural Parts with ForTii® Ace, Carburetor adapter heat shield insulation wall | |
Certifications | Yellow Card Available | |
Fillers | 50% Glass Fiber |