Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 1.35 % Show Supplier Material materials with Absorción de agua of 1.35 % | dry | ISO 62 | at 23°C after 24h |
4.8 % Show Supplier Material materials with Absorción de agua of 4.8 % | dry | Sim. to ISO 62 | ||
Densidad | 1.82 g/cm³ Show Supplier Material materials with Densidad of 1.82 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.2 % Show Supplier Material materials with Moisture absorption of 1.2 % | dry | Sim. to ISO 62 | |
Índice límite de óxigeno | 37 % Show Supplier Material materials with Índice límite de óxigeno of 37 % | dry | ISO 4589-1/-2 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 2 % Show Supplier Material materials with Elongación of 2 % | dry | ISO 527-1/-2 | |
3 % Show Supplier Material materials with Elongación of 3 % | conditioned | ISO 527-1/-2 | ||
120 °C | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 | |
160 °C | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 250 MPa Show Supplier Material materials with Flexural yield strength of 250 MPa | conditioned | ISO 178 | |
300 MPa Show Supplier Material materials with Flexural yield strength of 300 MPa | dry | ISO 178 | ||
120 °C | 230 MPa Show Supplier Material materials with Flexural yield strength of 230 MPa | dry | ISO 178 | |
160 °C | 200 MPa Show Supplier Material materials with Flexural yield strength of 200 MPa | dry | ISO 178 | |
Módulo de flexión | 11 GPa Show Supplier Material materials with Módulo de flexión of 11 GPa | conditioned | ISO 178 | |
15 GPa Show Supplier Material materials with Módulo de flexión of 15 GPa | dry | ISO 178 | ||
120 °C | 10.5 GPa Show Supplier Material materials with Módulo de flexión of 10.5 GPa | dry | ISO 178 | |
160 °C | 9 GPa Show Supplier Material materials with Módulo de flexión of 9 GPa | dry | ISO 178 | |
Módulo elástico | 12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | conditioned | ISO 527-1/-2 | |
17 GPa Show Supplier Material materials with Módulo elástico of 17 GPa | dry | ISO 527-1/-2 | ||
120 °C | 11 GPa Show Supplier Material materials with Módulo elástico of 11 GPa | dry | ISO 527-1/-2 | |
160 °C | 10 GPa Show Supplier Material materials with Módulo elástico of 10 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | 130 MPa Show Supplier Material materials with Resistencia a la tracción of 130 MPa | conditioned | ISO 527-1/-2 | |
200 MPa Show Supplier Material materials with Resistencia a la tracción of 200 MPa | dry | ISO 527-1/-2 | ||
120 °C | 130 MPa Show Supplier Material materials with Resistencia a la tracción of 130 MPa | dry | ISO 527-1/-2 | |
160 °C | 120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 13 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 13 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 14.0 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 14.0 kJ/m² | dry | ISO 179/1eA | |
23 °C | 15 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 15 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 50 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | dry | ISO 179/1eU | |
23 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
4.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 4.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 1.42e-07 mm²/s Show Supplier Material materials with Difusividad térmica of 1.42e-07 mm²/s | dry | - | |||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 825 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C | dry | IEC 60695-2-13 | 0.75 mm | ||
925 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 925 °C | dry | IEC 60695-2-13 | 3 mm | |||
Inflamabilidad | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 110 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 110 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 120 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 120 °C | dry | UL746B | 0.75 mm | ||
Temperatura de flexión bajo carga | 290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 295 °C Show Supplier Material materials with Temperatura de fusión of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperatura de reblandecimiento Vicat | 290 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 290 °C | dry | ISO 306 | 50°C/h 50N | ||
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
4.3 [-] Show Supplier Material materials with Constante dieléctrica of 4.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
12 [-] Show Supplier Material materials with Constante dieléctrica of 12 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 60 [-] Show Supplier Material materials with Factor de disipación of 60 [-] | dry | IEC 62631-2-1 | 100Hz |
160 [-] Show Supplier Material materials with Factor de disipación of 160 [-] | dry | IEC 62631-2-1 | 1MHz | |
700 [-] Show Supplier Material materials with Factor de disipación of 700 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3300 [-] Show Supplier Material materials with Factor de disipación of 3300 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 20 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 20 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+08 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+08 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 250 V Show Supplier Material materials with Índice de seguimiento comparativo of 250 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.3 % Show Supplier Material materials with Contracción of 0.3 % | dry | Sim. to ISO 294-4 | Parallel |
0.9 % Show Supplier Material materials with Contracción of 0.9 % | dry | Sim. to ISO 294-4 | Normal | |
Density of melt | 1710.0 g/cm³ Show Supplier Material materials with Density of melt of 1710.0 g/cm³ | dry | - | |
Specific heat capacity melt | 1530 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1530 J/(kg·K) | dry | - | |
Spiral flow length | 100 | dry | - | 1.0 mm 800 bar |
110 | dry | - | 1.0 mm 900 bar | |
120 | dry | - | 1.0 mm 1000 bar | |
Thermal conductivity of melt | 0.344 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.344 W/(m·K) | dry | - | |
Viscosity number | 140 cm³/gr Show Supplier Material materials with Viscosity number of 140 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Reflow connectors | |
Certifications | Yellow Card Available | |
Fillers | 45% Glass Fiber |