General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Absorción de agua | 9.5 % Show Supplier Material materials with Absorción de agua of 9.5 % | dry | Sim. to ISO 62 |
Densidad | 1.13 g/cm³ Show Supplier Material materials with Densidad of 1.13 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.5 % Show Supplier Material materials with Moisture absorption of 2.5 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 20 % Show Supplier Material materials with Elongación of 20 % | dry | ISO 527-1/-2 | |
50 % Show Supplier Material materials with Elongación of 50 % | conditioned | ISO 527-1/-2 | ||
Elongation at yield | 4 % Show Supplier Material materials with Elongation at yield of 4 % | dry | ISO 527-1/-2 | |
25 % Show Supplier Material materials with Elongation at yield of 25 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
Módulo de flexión | 2.6 GPa Show Supplier Material materials with Módulo de flexión of 2.6 GPa | dry | ISO 178 | |
Módulo elástico | 1 GPa Show Supplier Material materials with Módulo elástico of 1 GPa | conditioned | ISO 527-1/-2 | |
3.2 GPa Show Supplier Material materials with Módulo elástico of 3.2 GPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 2.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 2.5 kJ/m² | dry | ISO 179/1eA |
-30 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 4.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 35 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 35 kJ/m² | conditioned | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Difusividad térmica | 8.82e-08 mm²/s Show Supplier Material materials with Difusividad térmica of 8.82e-08 mm²/s | dry | - | |
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Density of melt | 960 g/cm³ Show Supplier Material materials with Density of melt of 960 g/cm³ | dry | - | |
Specific heat capacity melt | 2680 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2680 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.23 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.23 W/(m·K) | dry | - | |
Velocidad de flujo del volumen derretido | 230 °C | 15.2 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 15.2 cm³/10min | dry | ISO 1133 |
Viscosity number | 152 cm³/gr Show Supplier Material materials with Viscosity number of 152 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Certifications | Food Contact |