EN 1706 Grade AC-21100 T6

Want to keep this datasheet? Save it now in your required format

Description

Aluminium casting alloy (sand casting, permanent mould casting)

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.75 g/cm³

Show Material materials with Density of 2.75 g/cm³

T6

EN 1706

Casting

20.0 °C

2.75 g/cm³

Show Material materials with Density of 2.75 g/cm³

T6

EN 1706

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

80.0 - 110.0 MPa

Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa

T6

EN 1706

Casting

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T6

EN 1706

Casting

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T6

EN 1706

Hardness, Brinell

95.0 [-]

Show Material materials with Hardness, Brinell of 95.0 [-]

T6

EN 1706

Casting

20.0 °C

95.0 [-]

Show Material materials with Hardness, Brinell of 95.0 [-]

T6

EN 1706

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Cast 2xx.x Series Aluminium

Tensile strength

300.0 MPa

Show Material materials with Tensile strength of 300.0 MPa

T6

EN 1706

Casting

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T6

EN 1706

Casting

20.0 °C

300.0 MPa

Show Material materials with Tensile strength of 300.0 MPa

T6

EN 1706

20.0 °C

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T6

EN 1706

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

EN 1706

Casting

100.0 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

EN 1706

Casting

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

EN 1706

Casting

Melting point

540.0 - 640.0 °C

Show Material materials with Melting point of 540.0 - 640.0 °C

T6

EN 1706

Casting

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

T6

EN 1706

Casting

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

T6

EN 1706

Thermal conductivity

20.0 °C

120.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 150.0 W/(m·K)

T6

EN 1706

Casting

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

16000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 16000000.0 - 23000000.0 S/m

T6

EN 1706

Casting

Electrical resistivity

4.35e-08 - 6.25e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 6.25e-08 Ω·m

T6

EN 1706

Casting

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

93.4 %

Show Material materials with Aluminium of 93.4 %

T6

EN 1706

Copper

4.2 - 5.2 %

Show Material materials with Copper of 4.2 - 5.2 %

T6

EN 1706

Casting

Iron

0.19 %

Show Material materials with Iron of 0.19 %

T6

EN 1706

0.19 %

Show Material materials with Iron of 0.19 %

T6

EN 1706

Casting

Manganese

0.55 %

Show Material materials with Manganese of 0.55 %

T6

EN 1706

Casting

Silicon

0.18 %

Show Material materials with Silicon of 0.18 %

T6

EN 1706

Casting

Titanium

0.15 - 0.3 %

Show Material materials with Titanium of 0.15 - 0.3 %

T6

EN 1706

Casting

Zinc

0.07 %

Show Material materials with Zinc of 0.07 %

T6

EN 1706

Casting

Technological properties

Property
Anodizing

decorative: acceptable

Corrosion properties

general: not sufficient

General machinability

as cast: excellent

Processing methods

permanent mould casting, separately cast test sample