EN 1706 Grade AC-42200 T6

Want to keep this datasheet? Save it now in your required format

Description

Aluminium casting alloy (sand casting, permanent mould casting, investment casting)

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated Standards

Density

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

T6

EN 1706

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

80.0 - 110.0 MPa

Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa

T6

EN 1706, EN 13195

Casting

Elastic modulus

20.0 °C

69.0 - 75.0 GPa

Show Material materials with Elastic modulus of 69.0 - 75.0 GPa

T6

EN 1706

Hardness, Brinell

20.0 °C

85.0 [-]

Show Material materials with Hardness, Brinell of 85.0 [-]

T6

EN 1706

20.0 °C

100.0 [-]

Show Material materials with Hardness, Brinell of 100.0 [-]

T6

EN 1706

85.0 [-]

Show Material materials with Hardness, Brinell of 85.0 [-]

T6

EN 1706, EN 13195

Casting

100.0 [-]

Show Material materials with Hardness, Brinell of 100.0 [-]

T6

EN 1706, EN 13195

Casting

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Cast 3xx.x Series Aluminium

Shear modulus

2.8 GPa

Show Material materials with Shear modulus of 2.8 GPa

Typical for Cast 3xx.x Series Aluminium

Tensile strength

20.0 °C

290.0 MPa

Show Material materials with Tensile strength of 290.0 MPa

T6

EN 1706

20.0 °C

320.0 MPa

Show Material materials with Tensile strength of 320.0 MPa

T6

EN 1706

20.0 °C

250.0 MPa

Show Material materials with Tensile strength of 250.0 MPa

T6

EN 1706

250.0 MPa

Show Material materials with Tensile strength of 250.0 MPa

T6

EN 1706, EN 13195

Casting

290.0 MPa

Show Material materials with Tensile strength of 290.0 MPa

T6

EN 1706, EN 13195

Casting

320.0 MPa

Show Material materials with Tensile strength of 320.0 MPa

T6

EN 1706, EN 13195

Casting

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100.0 °C, 100 °C, 20 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

T6

EN 1706, EN 13195

Casting

Melting point

505.0 - 770.0 °C

Show Material materials with Melting point of 505.0 - 770.0 °C

Typical for Cast 3xx.x Series Aluminium

Specific heat capacity

960.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 960.0 - 963.0 J/(kg·K)

Typical for Cast 3xx.x Series Aluminium

Thermal conductivity

20.0 °C

150.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 150.0 - 180.0 W/(m·K)

T6

EN 1706, EN 13195

Casting

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 26000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 26000000.0 S/m

T6

EN 1706, EN 13195

Casting

Electrical resistivity

3.85e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 - 5e-08 Ω·m

T6

EN 1706, EN 13195

Casting

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

91.04 %

Show Material materials with Aluminium of 91.04 %

T6

EN 1706

Copper

0.05 %

Show Material materials with Copper of 0.05 %

T6

EN 1706, EN 13195

Casting

Iron

0.19 %

Show Material materials with Iron of 0.19 %

T6

EN 1706

0.19 %

Show Material materials with Iron of 0.19 %

T6

EN 1706, EN 13195

Casting

Magnesium

0.45 - 0.7 %

Show Material materials with Magnesium of 0.45 - 0.7 %

T6

EN 1706, EN 13195

Casting

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T6

EN 1706, EN 13195

Casting

Silicon

6.5 - 7.5 %

Show Material materials with Silicon of 6.5 - 7.5 %

T6

EN 1706, EN 13195

Casting

Titanium

0.08 - 0.25 %

Show Material materials with Titanium of 0.08 - 0.25 %

T6

EN 1706, EN 13195

Casting

Zinc

0.07 %

Show Material materials with Zinc of 0.07 %

T6

EN 1706, EN 13195

Casting

Technological properties

Property
Anodizing

decorative: not sufficient

Corrosion properties

general: good

General machinability

as cast: good

Processing methods

investment casting, separately cast test sample