General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Density | 2.65 g/cm³ Show Material materials with Density of 2.65 g/cm³ | F | EN 1706 | |
20.0 °C | 2.65 g/cm³ Show Material materials with Density of 2.65 g/cm³ | F | DIN 1725-2, EN 1676, EN 1706 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | ||
Elastic modulus | 75.0 GPa Show Material materials with Elastic modulus of 75.0 GPa | F | EN 1706 | ||
20.0 °C | 75.0 GPa Show Material materials with Elastic modulus of 75.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elongation | 5.0 % Show Material materials with Elongation of 5.0 % | F | EN 1706 | A50 | |
6.0 % Show Material materials with Elongation of 6.0 % | F | EN 1706 | A50 | ||
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 5.0 - 10.0 % Show Material materials with Elongation of 5.0 - 10.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 6.0 - 12.0 % Show Material materials with Elongation of 6.0 - 12.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Hardness, Brinell | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | F | EN 1706 | ||
55.0 [-] Show Material materials with Hardness, Brinell of 55.0 [-] | F | EN 1706 | |||
20.0 °C | 45.0 [-] Show Material materials with Hardness, Brinell of 45.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 45.0 - 60.0 [-] Show Material materials with Hardness, Brinell of 45.0 - 60.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 - 65.0 [-] Show Material materials with Hardness, Brinell of 50.0 - 65.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 4xx.x Series Aluminium | |||
Tensile strength | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F | EN 1706 | ||
170.0 MPa Show Material materials with Tensile strength of 170.0 MPa | F | EN 1706 | |||
20.0 °C | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 150.0 - 200.0 MPa Show Material materials with Tensile strength of 150.0 - 200.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Tensile strength of 170.0 - 230.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Thermal
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 1.9999999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.9999999999999998e-05 1/K | F | EN 1706 |
20 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
20 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | F | EN 1706 | |
100 °C | 1.9999999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.9999999999999998e-05 1/K | F | EN 1706 | |
200.0 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
200 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
300 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | F | EN 1706 | |
Melting point | 570.0 - 580.0 °C Show Material materials with Melting point of 570.0 - 580.0 °C | F | EN 1706 | |
Specific heat capacity | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Thermal conductivity | 140.0 - 170.0 W/(m·K) Show Material materials with Thermal conductivity of 140.0 - 170.0 W/(m·K) | F | EN 1706 | |
20.0 °C | 130.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 190.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 |
Electrical
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Electrical conductivity | 17000000.0 - 24000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 24000000.0 S/m | F | EN 1706 | |
20.0 °C | 17000000.0 - 26000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 26000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
Electrical resistivity | 4.17e-08 - 5.88e-08 Ω·m Show Material materials with Electrical resistivity of 4.17e-08 - 5.88e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 85.1 % Show Material materials with Aluminium of 85.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
0.50 % Show Material materials with Iron of 0.50 % | F | EN 1706 | |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Manganese | 0.001 - 0.4 % Show Material materials with Manganese of 0.001 - 0.4 % | F | DIN 1725-2, EN 1676, EN 1706 |
Silicon | 10.5 - 13.5 % Show Material materials with Silicon of 10.5 - 13.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: good | |
General machinability | after thermal treatment: acceptable | |
Processing methods | permanent mould casting, sample taken from casting or cast on |