General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Density | 2.65 g/cm³ Show Material materials with Density of 2.65 g/cm³ | F | EN 1706 | |
20.0 °C | 2.65 g/cm³ Show Material materials with Density of 2.65 g/cm³ | F | DIN 1725-2, EN 1676, EN 1706 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | F | EN 1706 | ||
Elastic modulus | 74.0 GPa Show Material materials with Elastic modulus of 74.0 GPa | F | EN 1706 | ||
20.0 °C | 74.0 GPa Show Material materials with Elastic modulus of 74.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elongation | 2.0 % Show Material materials with Elongation of 2.0 % | F | EN 1706 | A50 | |
2.5 % Show Material materials with Elongation of 2.5 % | F | EN 1706 | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.0 - 6.0 % Show Material materials with Elongation of 2.0 - 6.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Hardness, Brinell | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | F | EN 1706 | ||
55.0 [-] Show Material materials with Hardness, Brinell of 55.0 [-] | F | EN 1706 | |||
20.0 °C | 50.0 - 60.0 [-] Show Material materials with Hardness, Brinell of 50.0 - 60.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 - 80.0 [-] Show Material materials with Hardness, Brinell of 60.0 - 80.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Shear modulus | 2.8 GPa Show Material materials with Shear modulus of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Shear strength | 20.0 °C | 137.0 MPa Show Material materials with Shear strength of 137.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | |
Tensile strength | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F | EN 1706 | ||
180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | F | EN 1706 | |||
20.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 160.0 - 210.0 MPa Show Material materials with Tensile strength of 160.0 - 210.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 180.0 - 240.0 MPa Show Material materials with Tensile strength of 180.0 - 240.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Thermal
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | EN 1706 |
100 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | EN 1706 | |
200.0 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
Melting point | 550.0 - 600.0 °C Show Material materials with Melting point of 550.0 - 600.0 °C | F | EN 1706 | |
Specific heat capacity | 910.0 J/(kg·K) Show Material materials with Specific heat capacity of 910.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 910.0 J/(kg·K) Show Material materials with Specific heat capacity of 910.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Thermal conductivity | 150.0 - 170.0 W/(m·K) Show Material materials with Thermal conductivity of 150.0 - 170.0 W/(m·K) | F | EN 1706 | |
20.0 °C | 130.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 190.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 |
Electrical
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Electrical conductivity | 19000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 25000000.0 S/m | F | EN 1706 | |
20.0 °C | 17000000.0 - 26000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 26000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
Electrical resistivity | 4e-08 - 5.26e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 5.26e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 87.2 % Show Material materials with Aluminium of 87.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
0.50 % Show Material materials with Iron of 0.50 % | F | EN 1706 | |
Magnesium | 0.2 - 0.5 % Show Material materials with Magnesium of 0.2 - 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Manganese | 0.001 - 0.4 % Show Material materials with Manganese of 0.001 - 0.4 % | F | DIN 1725-2, EN 1676, EN 1706 |
Silicon | 9.0 - 11.0 % Show Material materials with Silicon of 9.0 - 11.0 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: good | |
General machinability | after thermal treatment: good to acceptable, as cast: good | |
Processing methods | permanent mould casting, sample taken from casting or cast on |