General
Property | Value | Comment |
---|---|---|
Density | 2.65 - 2.7 g/cm³ Show Material materials with Density of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanical
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastic modulus | 73.0 - 80.0 GPa Show Material materials with Elastic modulus of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Hardness, Brinell | 70.0 [-] Show Material materials with Hardness, Brinell of 70.0 [-] | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
95.0 [-] Show Material materials with Hardness, Brinell of 95.0 [-] | F | Pink Sheets, ASTM B108 | Casting | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Shear modulus | 2.8 GPa Show Material materials with Shear modulus of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Tensile strength | 160.0 MPa Show Material materials with Tensile strength of 160.0 MPa | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
185.0 MPa Show Material materials with Tensile strength of 185.0 MPa | F | Pink Sheets, ASTM B108 | Casting |
Thermal
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.3e-05 1/K | Typical for Cast 3xx.x Series Aluminium | |||
Melting point | 510.0 - 607.0 °C Show Material materials with Melting point of 510.0 - 607.0 °C | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting | |
Specific heat capacity | 960.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | |||
Thermal conductivity | 130.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Copper | 3.0 - 4.0 % Show Material materials with Copper of 3.0 - 4.0 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Iron | 1.00 % Show Material materials with Iron of 1.00 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Manganese | 0.5 % Show Material materials with Manganese of 0.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Nickel | 0.35 % Show Material materials with Nickel of 0.35 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Silicon | 5.5 - 6.5 % Show Material materials with Silicon of 5.5 - 6.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Titanium | 0.25 % Show Material materials with Titanium of 0.25 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Zinc | 1.0 % Show Material materials with Zinc of 1.0 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |