General
Property | Value | Comment |
---|---|---|
Density | 2.65 - 2.7 g/cm³ Show Material materials with Density of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanical
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastic modulus | 73.0 - 80.0 GPa Show Material materials with Elastic modulus of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Hardness, Brinell | 80.0 - 90.0 [-] Show Material materials with Hardness, Brinell of 80.0 - 90.0 [-] | T61 | Pink Sheets, ASTM B108 | Casting | |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Shear modulus | 2.8 GPa Show Material materials with Shear modulus of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Tensile strength | 195.0 MPa Show Material materials with Tensile strength of 195.0 MPa | T61 | Pink Sheets, ASTM B108 | Casting | |
230.0 MPa Show Material materials with Tensile strength of 230.0 MPa | T61 | Pink Sheets, ASTM B108 | Casting | ||
245.0 MPa Show Material materials with Tensile strength of 245.0 MPa | T61 | Pink Sheets, ASTM B26 | Casting | ||
260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | T61 | Pink Sheets, ASTM B108 | Casting |
Thermal
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.3e-05 1/K | Typical for Cast 3xx.x Series Aluminium | |||
Melting point | 557.0 - 613.0 °C Show Material materials with Melting point of 557.0 - 613.0 °C | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting | |
Specific heat capacity | 960.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | |||
Thermal conductivity | 130.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Copper | 0.2 % Show Material materials with Copper of 0.2 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |
Iron | 0.20 % Show Material materials with Iron of 0.20 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |
Magnesium | 0.25 - 0.45 % Show Material materials with Magnesium of 0.25 - 0.45 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |
Silicon | 6.5 - 7.5 % Show Material materials with Silicon of 6.5 - 7.5 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |
Titanium | 0.2 % Show Material materials with Titanium of 0.2 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T61 | Pink Sheets, ASTM B108, ASTM B26 | Casting |