General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 7.06 g/cm³ Show Supplier Material materials with Density of 7.06 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Charpy impact energy | 23.0 °C | 2.7 J Show Supplier Material materials with Charpy impact energy of 2.7 J | |
Compressive strength | 23.0 °C | 1448 MPa Show Supplier Material materials with Compressive strength of 1448 MPa | |
Compressive yield strength, 0.1% | 23.0 °C | 655 MPa Show Supplier Material materials with Compressive yield strength, 0.1% of 655 MPa | |
Elastic modulus | 23.0 °C | 103 GPa Show Supplier Material materials with Elastic modulus of 103 GPa | |
Elongation A5 | 23.0 °C | 0.5 % Show Supplier Material materials with Elongation A5 of 0.5 % | |
Hardness, HBW | 23.0 °C | 331 [-] Show Supplier Material materials with Hardness, HBW of 331 [-] | HBW 10/3000 |
Hardness, Rockwell C | 23.0 °C | 35 [-] Show Supplier Material materials with Hardness, Rockwell C of 35 [-] | |
Izod impact energy | 23.0 °C | 2.7 J Show Supplier Material materials with Izod impact energy of 2.7 J | |
Reduction of area | 23.0 °C | 0 % Show Supplier Material materials with Reduction of area of 0 % | |
Shear strength | 23.0 °C | 483 MPa Show Supplier Material materials with Shear strength of 483 MPa | |
Tensile strength | 23.0 °C | 586 MPa Show Supplier Material materials with Tensile strength of 586 MPa | |
Yield strength Rp0.2 | 23.0 °C | 489 MPa Show Supplier Material materials with Yield strength Rp0.2 of 489 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.62E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.62E-5 1/K |
Specific heat capacity | 23.0 °C | 420 J/(kg·K) Show Supplier Material materials with Specific heat capacity of 420 J/(kg·K) |
Thermal conductivity | 23.0 °C | 42 W/(m·K) Show Supplier Material materials with Thermal conductivity of 42 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical conductivity | 23.0 °C | 6.00E+6 S/m Show Supplier Material materials with Electrical conductivity of 6.00E+6 S/m |
Specific Electrical conductivity | 10 % IACS Show Supplier Material materials with Specific Electrical conductivity of 10 % IACS |
Chemical properties
Technological properties
Property | ||
---|---|---|
Application areas | The field of service of AMPCO® 22, with few exceptions, is limited to forming and/or drawing stainless steel, especially when runs are long or gauge is heavy and it is essential that tolerances are maintained. |