AMPCO-TRODE® 150 aluminum bronze spooled wire and bare filler rod produce a deposit of high strength and good ductility with a nominal hardness of 166 Brinell as applied with the inert-gas processes.


AMPCO-TRODE® 150 is recommended for welding AMPCO® 18 alloy. It is ideal for piston overlay applications and bearing surfaces requiring high strength and good ductility.

Related Standards

Equivalent Materials

This material data has been provided by AMPCO METAL.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyValue

Recycled Content

80 %

Show Supplier Material materials with Recycled Content of 80 %

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

20 %

Show Supplier Material materials with Elongation of 20 %

in 2″ (51 mm)

Hardness, Brinell

23.0 °C

166 [-]

Show Supplier Material materials with Hardness, Brinell of 166 [-]

BHN (3000kg) 1/4″ (6.4mm) deposit

Reduction of area

23.0 °C

22 %

Show Supplier Material materials with Reduction of area of 22 %

Tensile strength

23.0 °C

621 MPa

Show Supplier Material materials with Tensile strength of 621 MPa

Yield strength

23.0 °C

276 MPa

Show Supplier Material materials with Yield strength of 276 MPa

Chemical properties

PropertyValueComment

Aluminium

10 - 11.5 %

Show Supplier Material materials with Aluminium of 10 - 11.5 %

Copper

Balance, including silver

Iron

2 - 4.5 %

Show Supplier Material materials with Iron of 2 - 4.5 %

Other

0.5 %

Show Supplier Material materials with Other of 0.5 %

max.

Silicon

0.1 %

Show Supplier Material materials with Silicon of 0.1 %

max.

Technological properties

Property
Application areas

Welding: Hydraulic pistons, Bearing overlays, Impellers, Turbine runners, Press rams, Cable sheaves, Mill slippers, Valve seats and parts, Breaker blocks, Ceiling machine mandrels, Steel mill rolls, Welding AMPCO® 18