Mineral filled epoxy moulding compound with high temperature resistance and very good dimensional stability with Shelf life of 12 months at temperatures below 8°C
See where Epoxy NU 505 L falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.
Density
ρ2 g/cm³ at 20 °C
DIN 53479
Water absorption
cwater0.05 % at 20 °C
ISO 62, 100°C/30 min
Coefficient of thermal expansion
α1.8E-5 1/K at 20 °C
ISO 11359-2, Mean value for 20-105°C
Glass transition temperature
Tg200 °C
ISO 6721-7
Thermal conductivity
λ0.7 W/(m·K) at 20 °C
ISO 8894
Comparative tracking index
CTI300 V at 20 °C
IEC 60112
Dielectric constant, 50Hz
εr,50Hz5.5 [-] at 20 °C
IEC 60250
Electrical resistivity
ρel1.00E+13 Ω·m at 20 °C
IEC 60093
Loss tangent, 50Hz
tanδ50,Hz1.5 [-] at 20 °C
IEC 60250
Sheet resistivity
ρel,sheet16 Ω/sq at 20 °C
IEC 60093
Application areas
High precision parts for automotive-, electrical- and general engineering
Fillers
Mineral Powder
This material data has been provided by Duresco GmbH.