Properties

General

Density ρ

1.2 g/cm³ at 20 °C

ISO 1183 1

Water absorption cwater

0.15 % at 20 °C

ISO 62 4 (after storage in standard climate 23 °C/50% RH)

Water absorption, saturation cwater,sat

0.35 % at 20 °C

ISO 62 1 (after storage in water at 23 °C/50% RH until saturation 20 °C)

Mechanical

Elastic modulus E

2.4 GPa at 20 °C

ISO 527 2/1B/1

Elongation A

70 % at 20 °C

ISO 527 2/1B/50

Tensile strength Rm

60 MPa at 20 °C

ISO 527 2/1B/50

Yield strength YS

60 MPa at 20 °C

ISO 527 2/1B/50

Thermal

Coefficient of thermal expansion α

6.65E-5 1/K at 20 °C

DIN 53752 A

Heat deflection temperature, 1.80 MPa HDT1.8,MPa

127 °C

ISO 75-2/A

Max service temperature Tmax

120 °C

Thermal conductivity λ

0.2 W/(m·K) at 20 °C

DIN 52612

Vicat softening temperature Tsoft

148 °C

ISO 306, Method B50

Electrical

Dielectric constant, 1MHz εr,1MHz

3.1 [-] at 20 °C

IEC 60250

Dielectric strength EDS

35 kV/mm at 20 °C

IEC 60243 1

Dissipation factor, 1MHz ε''1MHz

5E-4 [-] at 20 °C

IEC 60250

Electrical resistivity ρel

1.00E+14 Ω·m at 20 °C

IEC 60093

Sheet resistivity ρel,sheet

1.00E+14 Ω/sq at 20 °C

IEC 60093

Optical

Refractive index nd

1.59 [-]

ISO 489

Technological properties

Application areas

Typical applications for Makrolon® GP sheets include machine guards, lighting fixtures, signs, wall and door partitions. The sheets offer protection against involuntary breakage and wilful destruction. Makrolon® GP sheets can be thermoformed, cold-curved and machined with ease.

This material data has been provided by Goodfellow.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.