General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.75 g/cm³ Show Material materials with Density of 2.75 g/cm³ | F | EN 1706 | Casting | |
20.0 °C | 2.75 g/cm³ Show Material materials with Density of 2.75 g/cm³ | F | EN 1706 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | Casting | ||
Elastic modulus | 75.0 GPa Show Material materials with Elastic modulus of 75.0 GPa | F | EN 1706 | Casting | ||
20.0 °C | 75.0 GPa Show Material materials with Elastic modulus of 75.0 GPa | F | EN 1706 | |||
Hardness, Brinell | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | F | EN 1706 | Casting | ||
75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | F | EN 1706 | Casting | |||
80.0 [-] Show Material materials with Hardness, Brinell of 80.0 [-] | F | EN 1706 | Casting | |||
20.0 °C | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | F | EN 1706 | |||
20.0 °C | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | F | EN 1706 | |||
20.0 °C | 80.0 [-] Show Material materials with Hardness, Brinell of 80.0 [-] | F | EN 1706 | |||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Shear modulus | 2.8 GPa Show Material materials with Shear modulus of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Tensile strength | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F | EN 1706 | Casting | ||
170.0 MPa Show Material materials with Tensile strength of 170.0 MPa | F | EN 1706 | Casting | |||
240.0 MPa Show Material materials with Tensile strength of 240.0 MPa | F | EN 1706 | Casting | |||
20.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F | EN 1706 | |||
20.0 °C | 170.0 MPa Show Material materials with Tensile strength of 170.0 MPa | F | EN 1706 | |||
20.0 °C | 240.0 MPa Show Material materials with Tensile strength of 240.0 MPa | F | EN 1706 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | EN 1706 | Casting |
100.0 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | EN 1706 | Casting | |
100 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | F | EN 1706 | Casting | |
Melting point | 490.0 - 600.0 °C Show Material materials with Melting point of 490.0 - 600.0 °C | F | EN 1706 | Casting | |
Specific heat capacity | 880.0 J/(kg·K) Show Material materials with Specific heat capacity of 880.0 J/(kg·K) | F | EN 1706 | Casting | |
20.0 °C | 880.0 J/(kg·K) Show Material materials with Specific heat capacity of 880.0 J/(kg·K) | F | EN 1706 | ||
Thermal conductivity | 20.0 °C | 110.0 - 130.0 W/(m·K) Show Material materials with Thermal conductivity of 110.0 - 130.0 W/(m·K) | F | EN 1706 | Casting |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 14000000.0 - 18000000.0 S/m Show Material materials with Electrical conductivity of 14000000.0 - 18000000.0 S/m | F | EN 1706 | Casting |
Electrical resistivity | 5.56e-08 - 7.14e-08 Ω·m Show Material materials with Electrical resistivity of 5.56e-08 - 7.14e-08 Ω·m | F | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 82.55 % Show Material materials with Aluminium of 82.55 % | F | EN 1706 | |
Copper | 2.0 - 3.5 % Show Material materials with Copper of 2.0 - 3.5 % | F | EN 1706 | Casting |
Iron | 0.8 % Show Material materials with Iron of 0.8 % | F | EN 1706 | |
0.80 % Show Material materials with Iron of 0.80 % | F | EN 1706 | Casting | |
Lead | 0.25 % Show Material materials with Lead of 0.25 % | F | EN 1706 | Casting |
Magnesium | 0.05 - 0.55 % Show Material materials with Magnesium of 0.05 - 0.55 % | F | EN 1706 | Casting |
Manganese | 0.15 - 0.65 % Show Material materials with Manganese of 0.15 - 0.65 % | F | EN 1706 | Casting |
Nickel | 0.35 % Show Material materials with Nickel of 0.35 % | F | EN 1706 | Casting |
Silicon | 7.5 - 9.5 % Show Material materials with Silicon of 7.5 - 9.5 % | F | EN 1706 | Casting |
Tin | 0.15 % Show Material materials with Tin of 0.15 % | F | EN 1706 | Casting |
Titanium | 0.25 % Show Material materials with Titanium of 0.25 % | F | EN 1706 | Casting |
Zinc | 1.2 % Show Material materials with Zinc of 1.2 % | F | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: not sufficient | |
General machinability | after thermal treatment: good | |
Processing methods | permanent mould casting, separately cast test sample |