G-AlSi12(Cu) is an eutectic alloy with excellent casting characteristics. It exhibits well plasticity with medium strength. The alloy is suitable for difficult shapes, thin-walled, pressure tight, oscillating loaded, impact loaded cast parts. It is excellently weldable. Application: devices, machines, vehicle and apparatus engineering, housing, impellers, rib body, equipment support

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated Standards

Density

2.65 g/cm³

Show Material materials with Density of 2.65 g/cm³

F

EN 1706

20.0 °C

2.65 g/cm³

Show Material materials with Density of 2.65 g/cm³

F

DIN 1725-2, EN 1676, EN 1706

Mechanical

PropertyTemperatureValueConditionRelated StandardsComment

Bending Fatigue Strength

60.0 - 90.0 MPa

Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa

F

EN 1706

Elastic modulus

75.0 GPa

Show Material materials with Elastic modulus of 75.0 GPa

F

EN 1706

20.0 °C

75.0 GPa

Show Material materials with Elastic modulus of 75.0 GPa

F

DIN 1725-2, EN 1676, EN 1706

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

F

EN 1706

A50

2.0 %

Show Material materials with Elongation of 2.0 %

F

EN 1706

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

F

DIN 1725-2, EN 1676, EN 1706

20.0 °C

1.0 - 4.0 %

Show Material materials with Elongation of 1.0 - 4.0 %

F

DIN 1725-2, EN 1676, EN 1706

20.0 °C

2.0 - 4.0 %

Show Material materials with Elongation of 2.0 - 4.0 %

F

DIN 1725-2, EN 1676, EN 1706

Hardness, Brinell

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

F

EN 1706

55.0 [-]

Show Material materials with Hardness, Brinell of 55.0 [-]

F

EN 1706

20.0 °C

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

F

DIN 1725-2, EN 1676, EN 1706

20.0 °C

50.0 - 65.0 [-]

Show Material materials with Hardness, Brinell of 50.0 - 65.0 [-]

F

DIN 1725-2, EN 1676, EN 1706

20.0 °C

55.0 - 75.0 [-]

Show Material materials with Hardness, Brinell of 55.0 - 75.0 [-]

F

DIN 1725-2, EN 1676, EN 1706

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Cast 3xx.x Series Aluminium

Shear modulus

2.8 GPa

Show Material materials with Shear modulus of 2.8 GPa

Typical for Cast 3xx.x Series Aluminium

Tensile strength

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

F

EN 1706

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

F

EN 1706

20.0 °C

140.0 MPa

Show Material materials with Tensile strength of 140.0 MPa

F

DIN 1725-2, EN 1676, EN 1706

20.0 °C

150.0 - 210.0 MPa

Show Material materials with Tensile strength of 150.0 - 210.0 MPa

F

DIN 1725-2, EN 1676, EN 1706

20.0 °C

180.0 - 240.0 MPa

Show Material materials with Tensile strength of 180.0 - 240.0 MPa

F

DIN 1725-2, EN 1676, EN 1706

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

20 °C

1.9999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.9999999999999998e-05 1/K

F

EN 1706

100 °C

1.9999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.9999999999999998e-05 1/K

F

EN 1706

200.0 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

F

DIN 1725-2, EN 1676, EN 1706

Melting point

530.0 - 580.0 °C

Show Material materials with Melting point of 530.0 - 580.0 °C

F

EN 1706

Specific heat capacity

890.0 J/(kg·K)

Show Material materials with Specific heat capacity of 890.0 J/(kg·K)

F

EN 1706

20.0 °C

890.0 J/(kg·K)

Show Material materials with Specific heat capacity of 890.0 J/(kg·K)

F

DIN 1725-2, EN 1676, EN 1706

Thermal conductivity

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

F

EN 1706

20.0 °C

120.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 160.0 W/(m·K)

F

DIN 1725-2, EN 1676, EN 1706

Electrical

PropertyTemperatureValueConditionRelated Standards

Electrical conductivity

16000000.0 - 22000000.0 S/m

Show Material materials with Electrical conductivity of 16000000.0 - 22000000.0 S/m

F

EN 1706

20.0 °C

15000000.0 - 22000000.0 S/m

Show Material materials with Electrical conductivity of 15000000.0 - 22000000.0 S/m

F

DIN 1725-2, EN 1676, EN 1706

Electrical resistivity

4.55e-08 - 6.25e-08 Ω·m

Show Material materials with Electrical resistivity of 4.55e-08 - 6.25e-08 Ω·m

F

EN 1706

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

82.6 %

Show Material materials with Aluminium of 82.6 %

F

DIN 1725-2, EN 1676, EN 1706

Copper

1.0 %

Show Material materials with Copper of 1.0 %

F

DIN 1725-2, EN 1676, EN 1706

Iron

0.8 %

Show Material materials with Iron of 0.8 %

F

DIN 1725-2, EN 1676, EN 1706

0.80 %

Show Material materials with Iron of 0.80 %

F

EN 1706

Lead

0.2 %

Show Material materials with Lead of 0.2 %

F

DIN 1725-2, EN 1676, EN 1706

Magnesium

0.3 %

Show Material materials with Magnesium of 0.3 %

F

DIN 1725-2, EN 1676, EN 1706

Manganese

0.1 - 0.5 %

Show Material materials with Manganese of 0.1 - 0.5 %

F

DIN 1725-2, EN 1676, EN 1706

Nickel

0.2

Show Material materials with Nickel of 0.2

F

DIN 1725-2, EN 1676, EN 1706

Silicon

10.5 - 13.5 %

Show Material materials with Silicon of 10.5 - 13.5 %

F

DIN 1725-2, EN 1676, EN 1706

Tin

0.1 %

Show Material materials with Tin of 0.1 %

F

DIN 1725-2, EN 1676, EN 1706

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

F

DIN 1725-2, EN 1676, EN 1706

Zinc

0.5 %

Show Material materials with Zinc of 0.5 %

F

DIN 1725-2, EN 1676, EN 1706

Technological properties

Property
Anodizing

decorative: not recommended

Corrosion properties

general: acceptable

General machinability

after thermal treatment: acceptable

Processing methods

permanent mould casting, separately cast test sample