Pink Sheets Grade 356.0 F

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by MakeItFrom.com,ASM Handbook Volume 2 Properties and Selection: Nonferrous oys and Special-Purpose Materials,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueCondition

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

F

72.4 GPa

Show Material materials with Elastic modulus of 72.4 GPa

F

Unlock all property charts

Elongation

3.8 %

Show Material materials with Elongation of 3.8 %

F

6 %

Show Material materials with Elongation of 6 %

F

Sand cast, elongation in 50 mm

Unlock all property charts

Elongation A100

23.0 °C

2 - 3 %

Show Material materials with Elongation A100 of 2 - 3 %

Hardness, Brinell

55.0 [-]

Show Material materials with Hardness, Brinell of 55.0 [-]

F

Pink Sheets, ASTM B26, ASTM B618

Casting

Unlock all property charts

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

F

Unlock all property charts

Shear modulus

27.2 GPa

Show Material materials with Shear modulus of 27.2 GPa

F

Unlock all property charts

Tensile strength

130.0 MPa

Show Material materials with Tensile strength of 130.0 MPa

F

Pink Sheets, ASTM B26, ASTM B618

Casting

164 MPa

Show Material materials with Tensile strength of 164 MPa

F

Sand cast

145.0 MPa

Show Material materials with Tensile strength of 145.0 MPa

F

Pink Sheets, ASTM B108

Casting

Unlock all property charts

Yield strength

100.0 MPa

Show Material materials with Yield strength of 100.0 MPa

F

124 MPa

Show Material materials with Yield strength of 124 MPa

F

Sand cast, RP02

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

F

Pink Sheets, ASTM B108

Casting

RP02

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

F

Pink Sheets, ASTM B26

Casting

RP02

Unlock all property charts

Yield strength Rp0.2

23.0 °C

65 - 124 MPa

Show Material materials with Yield strength Rp0.2 of 65 - 124 MPa

Sand cast

Thermal

PropertyValueConditionRelated StandardsShape

Coefficient of thermal expansion

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

F

Unlock all property charts

Melting point

570.0 °C

Show Material materials with Melting point of 570.0 °C

F

557.0 - 613.0 °C

Show Material materials with Melting point of 557.0 - 613.0 °C

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Specific heat capacity

970.0 J/(kg·K)

Show Material materials with Specific heat capacity of 970.0 J/(kg·K)

F

Unlock all property charts

Thermal conductivity

160.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 W/(m·K)

F

Unlock all property charts

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

90.1 - 93.3 %

Show Material materials with Aluminium of 90.1 - 93.3 %

F

Copper

0.25 %

Show Material materials with Copper of 0.25 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Iron

0.6 %

Show Material materials with Iron of 0.6 %

F

0.60 %

Show Material materials with Iron of 0.60 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Magnesium

0.2 - 0.45 %

Show Material materials with Magnesium of 0.2 - 0.45 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Manganese

0.35 %

Show Material materials with Manganese of 0.35 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Other

0.15 %

Show Material materials with Other of 0.15 %

F

Silicon

6.5 - 7.5 %

Show Material materials with Silicon of 6.5 - 7.5 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Titanium

0.25 %

Show Material materials with Titanium of 0.25 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting

Zinc

0.35 %

Show Material materials with Zinc of 0.35 %

F

Pink Sheets, ASTM B108, ASTM B26, ASTM B618

Casting