Epoxy NP500A - Sheet

Alternative and trade names
NEMA GRADE: G-10, U.L. LISTED: N
Want to keep this datasheet? Save it now in your required format

Description

NP500A is constructed of a woven glass fabric combined with easy-machining, non-brominated epoxy resin. It is engineered to provide NEMA grade G-10 properties, but is easier to machine and more cost effective in many applications. NP500A meets or exceeds the requirements of MIL-I-24768/2 and IEC 60893-2-EPGC 201.

This material data has been provided by Norplex Micarta.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Bonding strength

23.0 °C

1134 Kg

Show Supplier Material materials with Bonding strength of 1134 Kg

ASTM D229, Condition A

Density

23.0 °C

1.77 g/cm³

Show Supplier Material materials with Density of 1.77 g/cm³

ASTM D792

Moisture absorption

23.0 °C

0.22 %

Show Supplier Material materials with Moisture absorption of 0.22 %

ASTM D570, Condition D₁-24/23

Mechanical

PropertyTemperatureValueComment

Compressive strength

23.0 °C

433 MPa

Show Supplier Material materials with Compressive strength of 433 MPa

ASTM D695, Condition A, Flatwise

Flexural modulus

23.0 °C

23.4 GPa

Show Supplier Material materials with Flexural modulus of 23.4 GPa

ASTM D790, Condition A

Flexural modulus, transverse

23.0 °C

22.8 GPa

Show Supplier Material materials with Flexural modulus, transverse of 22.8 GPa

ASTM D790, Condition A

Flexural strength

23.0 °C

455.1 MPa

Show Supplier Material materials with Flexural strength of 455.1 MPa

ASTM D790, Condition A

Flexural strength, transverse

23.0 °C

413.7 MPa

Show Supplier Material materials with Flexural strength, transverse of 413.7 MPa

ASTM D790, Condition A

Hardness, Rockwell M

23.0 °C

99 [-]

Show Supplier Material materials with Hardness, Rockwell M of 99 [-]

ASTM D785

Impact strength, Izod unnotched, ASTM

23.0 °C

507 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 507 J/m

ASTM D256, Condition E-48/50

Impact strength, Izod unnotched, ASTM, Transversal

23.0 °C

400 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM, Transversal of 400 J/m

ASTM D256, Condition E-48/50

Shear strength, transverse

23.0 °C

131 MPa

Show Supplier Material materials with Shear strength, transverse of 131 MPa

ASTM D732, Condition A

Tensile strength

23.0 °C

296.5 MPa

Show Supplier Material materials with Tensile strength of 296.5 MPa

ASTM D638, Condition A

Tensile strength, transverse

23.0 °C

268.9 MPa

Show Supplier Material materials with Tensile strength, transverse of 268.9 MPa

ASTM D638, Condition A

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.21E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

IPC-TM 650-2.4.24

Coefficient of thermal expansion, transverse

23.0 °C

9.6E-6 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 9.6E-6 1/K

IPC-TM 650-2.4.24

Glass transition temperature

120 °C

Show Supplier Material materials with Glass transition temperature of 120 °C

DMA

Relative temperature index, electrical

130 °C

Show Supplier Material materials with Relative temperature index, electrical of 130 °C

UL Bulletin 746b¹

Relative temperature index, mechanical strength

140 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C

UL Bulletin 746b¹

Flammability

UL Bulletin 94, Class HB

Electrical

PropertyTemperatureValueComment

Breakdown voltage

23.0 °C

48 - 49 kV

Show Supplier Material materials with Breakdown voltage of 48 - 49 kV

ASTM D149, Condition A (Min.) & D-48/50 (Max.)

Dielectric strength

23.0 °C

27.17 kV/mm

Show Supplier Material materials with Dielectric strength of 27.17 kV/mm

ASTM D149, Condition A & D-48/50

Technological properties

Property
Application areas

Applications for NP500A include: low temperature thermal insulation, structural applications and various other mechanical, and electrical applications at low to moderately high temperatures.

Fillers

Glass Fabric

Other

1.This temperature is a recommendation only, and based upon experience in various applications. The maximum operating temperature is dependent upon the application and should be investigated prior to use.

Supplier Disclaimer

This data, while believed to be accurate and based on reliable analytical methods, is for informational purposes only. The terms and conditions of the agreement under which it is sold will govern any sales of this product. Data supplied above are "typical values"; not to be considered "specification values".


To assure the material's performance is adequate for a specific application; customers should verify, independent of Norplex-Micarta, performance characteristics of interest.


It is the responsibility of the users of this information to make sure that they have the latest version of this TDB, and are urged to check with Customer Service or, preferably our web site, www.norplex-micarta.com, to determine if the information is the most current available.