Phenolic NP515LS - Sheet

Alternative and trade names
NEMA GRADE: G-3, U.L. LISTED: N
Want to keep this datasheet? Save it now in your required format

Description

NP515LS is a woven glass fabric combined with a high temperature phenolic resin. It is engineered to provide superior shrink characteristics at elevated temperatures, making it an ideal material for insulating gaskets. Having been tested and certified as a NEMA G-3 material, NP515LS also meets or exceeds the requirements of IEC 60893-3-4 PF GC 201.

This material data has been provided by Norplex Micarta.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Bonding strength

23.0 °C

725.74 Kg

Show Supplier Material materials with Bonding strength of 725.74 Kg

Condition A

Density

23.0 °C

1.89 g/cm³

Show Supplier Material materials with Density of 1.89 g/cm³

Moisture absorption

23.0 °C

0.56 %

Show Supplier Material materials with Moisture absorption of 0.56 %

Mechanical

PropertyTemperatureValueComment

Compressive strength

23.0 °C

526.76 MPa

Show Supplier Material materials with Compressive strength of 526.76 MPa

Flatwise

Flexural strength

23.0 °C

484.01 MPa

Show Supplier Material materials with Flexural strength of 484.01 MPa

Flexural strength, transverse

23.0 °C

338.53 MPa

Show Supplier Material materials with Flexural strength, transverse of 338.53 MPa

Hardness, Rockwell M

23.0 °C

112 [-]

Show Supplier Material materials with Hardness, Rockwell M of 112 [-]

Impact strength, Izod notched, ASTM

23.0 °C

731.3 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 731.3 J/m

Impact strength, Izod notched, ASTM, Transversal

23.0 °C

453.7 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM, Transversal of 453.7 J/m

Tensile strength

23.0 °C

378.52 MPa

Show Supplier Material materials with Tensile strength of 378.52 MPa

Thermal

PropertyValue

Flammability

UL 94, Class HB

Technological properties

Property
Application areas

Insulating gaskets

Fillers

Glass Fabric

Other

The mechanical properties are converted from American unit system to International unit system.

Supplier Disclaimer

This data, while believed to be accurate and based on reliable analytical methods, is for informational purposes only. The terms and conditions of the agreement under which it is sold will govern any sales of this product. Data supplied above are "typical values"; not to be considered "specification values".


To assure the material's performance is adequate for a specific application; customers should verify, independent of Norplex-Micarta, performance characteristics of interest.


It is the responsibility of the users of this information to make sure that they have the latest version of this TDB, and are urged to check with Customer Service or, preferably our web site, www.norplex-micarta.com, to determine if the information is the most current available.