Description

NP575 is a woven glass fabric combined with a high temperature epoxy resin. It is engineered to provide superior characteristics at elevated temperatures.

This material data has been provided by Norplex Micarta.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Moisture absorption

23.0 °C

0.07 %

Show Supplier Material materials with Moisture absorption of 0.07 %

ASTM D570, Condition D₁-24/23

Mechanical

PropertyTemperatureValueComment

Compressive strength

130.0 °C

482.6 MPa

Show Supplier Material materials with Compressive strength of 482.6 MPa

ASTM D695

140.0 °C

462 MPa

Show Supplier Material materials with Compressive strength of 462 MPa

ASTM D695

155.0 °C

496.4 MPa

Show Supplier Material materials with Compressive strength of 496.4 MPa

ASTM D695

Flexural strength

20.0 °C

441 MPa

Show Supplier Material materials with Flexural strength of 441 MPa

ASTM D790

130.0 °C

420.6 MPa

Show Supplier Material materials with Flexural strength of 420.6 MPa

ASTM D790

140.0 °C

417.1 MPa

Show Supplier Material materials with Flexural strength of 417.1 MPa

ASTM D790

155.0 °C

365.2 MPa

Show Supplier Material materials with Flexural strength of 365.2 MPa

ASTM D790

Unlock all property charts

Flexural strength, transverse

23.0 °C

448.16 MPa

Show Supplier Material materials with Flexural strength, transverse of 448.16 MPa

ASTM D790, Condition A

Impact strength, Izod unnotched, ASTM

23.0 °C

1494 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 1494 J/m

ASTM D256, Condition E-48/50

Impact strength, Izod unnotched, ASTM, Transversal

23.0 °C

1227 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM, Transversal of 1227 J/m

ASTM D256, Condition E-48/50

Electrical

PropertyTemperatureValueComment

Breakdown voltage

23.0 °C

55 - 75 kV

Show Supplier Material materials with Breakdown voltage of 55 - 75 kV

ASTM D149, Condition D-48/50 (Min.) & A (Max.)

Dielectric constant, 1MHz

23.0 °C

4.8 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 4.8 [-]

ASTM D150

Dissipation factor, 1MHz

23.0 °C

0.03 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 0.03 [-]

ASTM D150

Electrical resistivity

23.0 °C

6.90E+11 Ω·m

Show Supplier Material materials with Electrical resistivity of 6.90E+11 Ω·m

ASTM D257

Surface resistivity

23.0 °C

2.30E+15 Ω/sq

Show Supplier Material materials with Surface resistivity of 2.30E+15 Ω/sq

ASTM D257

Technological properties

Property
Application areas

Ideal material for retaining ring insulation.

Fillers

Glass Fabric

Other

The mechanical properties are converted from American unit system to International unit system.

Supplier Disclaimer

This data, while believed to be accurate and based on reliable analytical methods, is for informational purposes only. The terms and conditions of the agreement under which it is sold will govern any sales of this product. Data supplied above are "typical values"; not to be considered "specification values".


To assure the material's performance is adequate for a specific application; customers should verify, independent of Norplex-Micarta, performance characteristics of interest.


It is the responsibility of the users of this information to make sure that they have the latest version of this TDB, and are urged to check with Customer Service or, preferably our web site, www.norplex-micarta.com, to determine if the information is the most current available.