General
Property | Value | Temperature | Comment |
---|---|---|---|
Bonding strength | 635 Kg Show Supplier Material materials with Bonding strength of 635 Kg at 23.0 °C | 23.0 °C | ASTM D229, Condition A |
Density | 1.38 g/cm³ Show Supplier Material materials with Density of 1.38 g/cm³ at 23.0 °C | 23.0 °C | ASTM D792 |
Moisture absorption | 3.2 % Show Supplier Material materials with Moisture absorption of 3.2 % at 23.0 °C | 23.0 °C | ASTM D570, Condition Dᵢ-24/23 |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Compressive strength | 186.2 MPa Show Supplier Material materials with Compressive strength of 186.2 MPa at 23.0 °C | 23.0 °C | ASTM D695, Condition A, Flatwise |
Flexural modulus | 6.9 GPa Show Supplier Material materials with Flexural modulus of 6.9 GPa at 23.0 °C | 23.0 °C | ASTM D790, Condition A |
Flexural modulus, transverse | 5.9 GPa Show Supplier Material materials with Flexural modulus, transverse of 5.9 GPa at 23.0 °C | 23.0 °C | ASTM D790, Condition A |
Flexural strength | 133.1 MPa Show Supplier Material materials with Flexural strength of 133.1 MPa at 23.0 °C | 23.0 °C | ASTM D790, Condition A |
Flexural strength, transverse | 121.3 MPa Show Supplier Material materials with Flexural strength, transverse of 121.3 MPa at 23.0 °C | 23.0 °C | ASTM D790, Condition A |
Hardness, Rockwell M | 84 [-] Show Supplier Material materials with Hardness, Rockwell M of 84 [-] at 23.0 °C | 23.0 °C | ASTM D785 |
Impact strength, Izod unnotched, ASTM | 41 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 41 J/m at 23.0 °C | 23.0 °C | ASTM D256, Condition E-48/50 |
Impact strength, Izod unnotched, ASTM, Transversal | 35 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM, Transversal of 35 J/m at 23.0 °C | 23.0 °C | ASTM D256, Condition E-48/50 |
Shear strength, transverse | 65.5 MPa Show Supplier Material materials with Shear strength, transverse of 65.5 MPa at 23.0 °C | 23.0 °C | ASTM D732, Condition A |
Tensile strength | 86.2 MPa Show Supplier Material materials with Tensile strength of 86.2 MPa at 23.0 °C | 23.0 °C | ASTM D638, Condition A |
Tensile strength, transverse | 57.9 MPa Show Supplier Material materials with Tensile strength, transverse of 57.9 MPa at 23.0 °C | 23.0 °C | ASTM D638, Condition A |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Arc resistance | 110 seconds, ASTM D495, Condition A | ||
Coefficient of thermal expansion | 1.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.5E-5 1/K at 23.0 °C | 23.0 °C | IPC-TM 650-2.4.24 |
Coefficient of thermal expansion, transverse | 1.9E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 1.9E-5 1/K at 23.0 °C | 23.0 °C | IPC-TM 650-2.4.24 |
Flammability | UL Bulletin 94, Class HB, Condition A | ||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | UL Bulletin 746b¹ | |
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | UL Bulletin 746b¹ |
Electrical
Property | Value | Temperature | Comment |
---|---|---|---|
Breakdown voltage | 10 - 55 kV Show Supplier Material materials with Breakdown voltage of 10 - 55 kV at 23.0 °C | 23.0 °C | ASTM D149, Condition D48/50 (Min.) & A (Max.) |
Comparative tracking index | 500 V Show Supplier Material materials with Comparative tracking index of 500 V at 23.0 °C | 23.0 °C | ASTM D3638 |
Dielectric constant, 1MHz | 5.5 [-] Show Supplier Material materials with Dielectric constant, 1MHz of 5.5 [-] at 23.0 °C | 23.0 °C | ASTM D150, Condition D-24/23 |
Dielectric strength | 27.56 kV/mm Show Supplier Material materials with Dielectric strength of 27.56 kV/mm at 23.0 °C | 23.0 °C | ASTM D149, Condition A |
Dissipation factor, 1MHz | 0.06 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 0.06 [-] at 23.0 °C | 23.0 °C | ASTM D150, Condition D-24/23 |
Technological properties
Property | ||
---|---|---|
Fillers | Paper | |
Other | 1.This temperature is a recommendation only, and based upon experience in various applications. The maximum operating temperature is dependent upon the application and should be investigated prior to use | |
Supplier Disclaimer | This data, while believed to be accurate and based on reliable analytical methods, is for informational purposes only. The terms and conditions of the agreement under which it is sold will govern any sales of this product. Data supplied above are "typical values"; not to be considered "specification values". To assure the material's performance is adequate for a specific application; customers should verify, independent of Norplex-Micarta, performance characteristics of interest. It is the responsibility of the users of this information to make sure that they have the latest version of this TDB, and are urged to check with Customer Service or, preferably our web site, www.norplex-micarta.com, to determine if the information is the most current available. |