Description

17 oz. aramid and "soft glass" fibers are combined to make a fabric that is stronger than pure aramid and less abrasive than glass fabrics. This material is impregnated with a high temperature epoxy resin matrix, which produces a composite with excellent mechanical strength at elevated temperatures and adverse environments.

This material data has been provided by Norplex Micarta.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Bonding strength

23.0 °C

1134 Kg

Show Supplier Material materials with Bonding strength of 1134 Kg

ASTM D229, Condition A

Density

23.0 °C

1.42 g/cm³

Show Supplier Material materials with Density of 1.42 g/cm³

ASTM D792

Moisture absorption

23.0 °C

0.23 %

Show Supplier Material materials with Moisture absorption of 0.23 %

ASTM D570, Condition Dᵢ-24/23

Mechanical

PropertyTemperatureValueComment

Compressive strength

23.0 °C

190.3 MPa

Show Supplier Material materials with Compressive strength of 190.3 MPa

ASTM D695, Condition A, Flatwise

Flexural modulus

23.0 °C

12.4 GPa

Show Supplier Material materials with Flexural modulus of 12.4 GPa

ASTM D790, Condition A

Flexural modulus, transverse

23.0 °C

11.7 GPa

Show Supplier Material materials with Flexural modulus, transverse of 11.7 GPa

ASTM D790, Condition A

Flexural strength

23.0 °C

232.4 - 284.8 MPa

Show Supplier Material materials with Flexural strength of 232.4 - 284.8 MPa

ASTM D790, Condition E-1/150: T-150 (Min.) & A (Max.)

Flexural strength, transverse

23.0 °C

111 - 131.7 MPa

Show Supplier Material materials with Flexural strength, transverse of 111 - 131.7 MPa

ASTM D790, Condition E-1/150: T-150 (Min.) & A (Max.)

Hardness, Rockwell M

23.0 °C

100 [-]

Show Supplier Material materials with Hardness, Rockwell M of 100 [-]

ASTM D785

Impact strength, Izod unnotched, ASTM

23.0 °C

694 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 694 J/m

ASTM D256, Condition A

Impact strength, Izod unnotched, ASTM, Transversal

23.0 °C

480 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM, Transversal of 480 J/m

ASTM D256, Condition A

Shear strength, transverse

23.0 °C

117.2 MPa

Show Supplier Material materials with Shear strength, transverse of 117.2 MPa

Tensile strength

23.0 °C

180.6 MPa

Show Supplier Material materials with Tensile strength of 180.6 MPa

ASTM D638, Condition A

Tensile strength, transverse

23.0 °C

62.7 MPa

Show Supplier Material materials with Tensile strength, transverse of 62.7 MPa

ASTM D638, Condition A

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

4.44E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 4.44E-5 1/K

IPC-TM 650-2.4.24

Coefficient of thermal expansion, transverse

23.0 °C

2.6E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 2.6E-5 1/K

IPC-TM 650-2.4.24

Relative temperature index, mechanical strength

180 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 180 °C

UL Bulletin 746b¹

Flammability

UL Bulletin 94, Class HB, Condition A

Technological properties

Property
Fillers

Aramid Fiber

Other

1.This temperature is a recommendation only, and based upon experience in various applications. The maximum operating temperature is dependent upon the application and should be investigated prior to use

Supplier Disclaimer

This data, while believed to be accurate and based on reliable analytical methods, is for informational purposes only. The terms and conditions of the agreement under which it is sold will govern any sales of this product. Data supplied above are "typical values"; not to be considered "specification values".


To assure the material's performance is adequate for a specific application; customers should verify, independent of Norplex-Micarta, performance characteristics of interest.


It is the responsibility of the users of this information to make sure that they have the latest version of this TDB, and are urged to check with Customer Service or, preferably our web site, www.norplex-micarta.com, to determine if the information is the most current available.