Radel® PPSU MS NT1 AM Filament

Want to keep this datasheet? Save it now in your required format

Description

Radel® MS NT1 AM Filament offers the best of sulfone polymers, with a superiority in both toughness and impact strength, high temperature capabilities, as well as proven outperformance in chemical resistance relative to both PSU and PEI. It enables applications in Aerospace, Healthcare, Smart Devices, and Energy Storage.

This material data has been provided by Solvay Specialty Polymers.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.29 g/cm³

Show Supplier Material materials with Density of 1.29 g/cm³

ASTM D792

Dimension

PropertyValue

Diameter

1.75 mm

Show Supplier Material materials with Diameter of 1.75 mm

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2 GPa

Show Supplier Material materials with Elastic modulus of 2 GPa

ASTM D638

Elongation

23.0 °C

21 %

Show Supplier Material materials with Elongation of 21 %

ASTM D638

Elongation at yield

23.0 °C

7 %

Show Supplier Material materials with Elongation at yield of 7 %

ASTM D638

Impact strength, Izod notched, ASTM

23.0 °C

480 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 480 J/m

ASTM D256

Tensile strength

23.0 °C

42 MPa

Show Supplier Material materials with Tensile strength of 42 MPa

ASTM D638

Yield strength

23.0 °C

62 MPa

Show Supplier Material materials with Yield strength of 62 MPa

ASTM D638

Thermal

PropertyValueComment

Glass transition temperature

220 °C

Show Supplier Material materials with Glass transition temperature of 220 °C

DSC

Technological properties

Property
Application areas

Aerospace Applications, Additive Manufacturing (3D Printing), Energy Storage, Medical/Healthcare applications, Smart Devices

Certifications

Substances used to manufacture the polymer grade used for this filament meets the requirements of Commission Regulation (EU) N°10/2011, which implements the framework regulation EU 1935/2004 as related to plastic materials and articles intended to come into contact with food and its subsequent amendments as well as the GMP requirements for EU 2023/2006.


Please feel free to contact the supplier for RoHS Compliance.

Color

Natural

Features

  • Acid Resistant
  • Base Resistant
  • Chemical Resistant
  • Flame Retardant
  • Good Impact Resistance
  • Good Thermal Stability
  • High Heat Resistance
  • Ultra High Toughness
  • Other

    Test specimen parameters:

  • First layer: 0.3mm thick
  • Subsequent layers: 0.1mm
  • 100% infill
  • 3 shells
  • Printing speed: 18 mm/s

  • Note:

    Typical properties: these are not to be construed as specifications

    Processing methods

    Fused Filament Fabrication (FFF)


    Printing conditions for above data table:

  • Filament drying conditions, minimum temperature 4h: 150°C
  • Extruder temperature: 380-410°C
  • Bed temperature: 180-220°C