General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Density | 20.0 °C | 2.65 g/cm³ Show Material materials with Density of 2.65 g/cm³ | T1 | DIN 1725-2, EN 1676, EN 1706 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 75.0 GPa Show Material materials with Elastic modulus of 75.0 GPa | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Elongation | 20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | T1 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 6.0 - 12.0 % Show Material materials with Elongation of 6.0 - 12.0 % | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
Hardness, Brinell | 20.0 °C | 45.0 [-] Show Material materials with Hardness, Brinell of 45.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 45.0 - 60.0 [-] Show Material materials with Hardness, Brinell of 45.0 - 60.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 - 65.0 [-] Show Material materials with Hardness, Brinell of 50.0 - 65.0 [-] | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 4xx.x Series Aluminium | |||
Tensile strength | 20.0 °C | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 150.0 - 200.0 MPa Show Material materials with Tensile strength of 150.0 - 200.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 160.0 MPa Show Material materials with Tensile strength of 160.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Tensile strength of 170.0 - 230.0 MPa | T1 | DIN 1725-2, EN 1676, EN 1706 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 200.0 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Melting point | 565.0 - 630.0 °C Show Material materials with Melting point of 565.0 - 630.0 °C | Typical for Cast 4xx.x Series Aluminium | |||
Specific heat capacity | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | T1 | DIN 1725-2, EN 1676, EN 1706 | |
Thermal conductivity | 20.0 °C | 130.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 190.0 W/(m·K) | T1 | DIN 1725-2, EN 1676, EN 1706 |
Electrical
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Electrical conductivity | 20.0 °C | 17000000.0 - 26000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 26000000.0 S/m | T1 | DIN 1725-2, EN 1676, EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 85.1 % Show Material materials with Aluminium of 85.1 % | T1 | DIN 1725-2, EN 1676, EN 1706 |
Copper | 0.05 Show Material materials with Copper of 0.05 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Iron | 0.5 Show Material materials with Iron of 0.5 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Magnesium | 0.05 Show Material materials with Magnesium of 0.05 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Manganese | 0.001 - 0.4 % Show Material materials with Manganese of 0.001 - 0.4 % | T1 | DIN 1725-2, EN 1676, EN 1706 |
Silicon | 10.5 - 13.5 % Show Material materials with Silicon of 10.5 - 13.5 % | T1 | DIN 1725-2, EN 1676, EN 1706 |
Titanium | 0.15 Show Material materials with Titanium of 0.15 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.1 Show Material materials with Zinc of 0.1 | T1 | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting, sample taken from casting or cast on |