G-AlCu4Ti - solidifies in an wide range of temperature - complicated casting - application in part hardend or warm hardend state - applicable for simple cast pieces, with high demands to strength and toughness application: - wear resistant construction parts in automobile, machine and aircraft industry

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated Standards

Density

20.0 °C

2.75 g/cm³

Show Material materials with Density of 2.75 g/cm³

T61

DIN 1725-2, EN 1676, EN 1706

Mechanical

PropertyTemperatureValueConditionRelated StandardsComment

Elastic modulus

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T61

DIN 1725-2, EN 1676, EN 1706

Elongation

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

5.0 - 10.0 %

Show Material materials with Elongation of 5.0 - 10.0 %

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

8.0 - 18.0 %

Show Material materials with Elongation of 8.0 - 18.0 %

T61

DIN 1725-2, EN 1676, EN 1706

Hardness, Brinell

20.0 °C

80.0 [-]

Show Material materials with Hardness, Brinell of 80.0 [-]

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

85.0 [-]

Show Material materials with Hardness, Brinell of 85.0 [-]

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

85.0 - 105.0 [-]

Show Material materials with Hardness, Brinell of 85.0 - 105.0 [-]

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

90.0 - 105.0 [-]

Show Material materials with Hardness, Brinell of 90.0 - 105.0 [-]

T61

DIN 1725-2, EN 1676, EN 1706

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Cast 2xx.x Series Aluminium

Tensile strength

20.0 °C

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

260.0 MPa

Show Material materials with Tensile strength of 260.0 MPa

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

280.0 - 380.0 MPa

Show Material materials with Tensile strength of 280.0 - 380.0 MPa

T61

DIN 1725-2, EN 1676, EN 1706

20.0 °C

320.0 - 400.0 MPa

Show Material materials with Tensile strength of 320.0 - 400.0 MPa

T61

DIN 1725-2, EN 1676, EN 1706

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

200.0 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T61

DIN 1725-2, EN 1676, EN 1706

Melting point

510.0 - 790.0 °C

Show Material materials with Melting point of 510.0 - 790.0 °C

Typical for Cast 2xx.x Series Aluminium

Specific heat capacity

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

T61

DIN 1725-2, EN 1676, EN 1706

Thermal conductivity

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 140.0 W/(m·K)

T61

DIN 1725-2, EN 1676, EN 1706

Electrical

PropertyTemperatureValueConditionRelated StandardsComment

Electrical conductivity

20.0 °C

16000000.0 - 20000000.0 S/m

Show Material materials with Electrical conductivity of 16000000.0 - 20000000.0 S/m

T61

DIN 1725-2, EN 1676, EN 1706

Electrical resistivity

4.347826086956522e-08 - 6.25e-08 Ω·m

Show Material materials with Electrical resistivity of 4.347826086956522e-08 - 6.25e-08 Ω·m

Typical for Cast 2xx.x Series Aluminium

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

93.5 %

Show Material materials with Aluminium of 93.5 %

T61

DIN 1725-2, EN 1676, EN 1706

Copper

4.5 - 5.2 %

Show Material materials with Copper of 4.5 - 5.2 %

T61

DIN 1725-2, EN 1676, EN 1706

Iron

0.18

Show Material materials with Iron of 0.18

T61

DIN 1725-2, EN 1676, EN 1706

Manganese

0.001 - 0.5 %

Show Material materials with Manganese of 0.001 - 0.5 %

T61

DIN 1725-2, EN 1676, EN 1706

Silicon

0.18

Show Material materials with Silicon of 0.18

T61

DIN 1725-2, EN 1676, EN 1706

Titanium

0.15 - 0.3 %

Show Material materials with Titanium of 0.15 - 0.3 %

T61

DIN 1725-2, EN 1676, EN 1706

Zinc

0.07

Show Material materials with Zinc of 0.07

T61

DIN 1725-2, EN 1676, EN 1706

Technological properties

Property
Processing methods

permanent mould casting, sample taken from casting