Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Density | 20.0 °C | 2.75 g/cm³ Show Material materials with Density of 2.75 g/cm³ | T5 | DIN 1725-2, EN 1676, EN 1706 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 72.0 GPa Show Material materials with Elastic modulus of 72.0 GPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Elongation | 20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 3.0 - 8.0 % Show Material materials with Elongation of 3.0 - 8.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 7.0 - 12.0 % Show Material materials with Elongation of 7.0 - 12.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Hardness, Brinell | 20.0 °C | 90.0 [-] Show Material materials with Hardness, Brinell of 90.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 95.0 - 110.0 [-] Show Material materials with Hardness, Brinell of 95.0 - 110.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 2xx.x Series Aluminium | |||
Tensile strength | 20.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 280.0 MPa Show Material materials with Tensile strength of 280.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 300.0 - 380.0 MPa Show Material materials with Tensile strength of 300.0 - 380.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 330.0 - 400.0 MPa Show Material materials with Tensile strength of 330.0 - 400.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 200.0 °C | 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Melting point | 510.0 - 790.0 °C Show Material materials with Melting point of 510.0 - 790.0 °C | Typical for Cast 2xx.x Series Aluminium | |||
Specific heat capacity | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Thermal conductivity | 20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Thermal conductivity of 110.0 - 140.0 W/(m·K) | T5 | DIN 1725-2, EN 1676, EN 1706 |
Electrical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 16000000.0 - 20000000.0 S/m Show Material materials with Electrical conductivity of 16000000.0 - 20000000.0 S/m | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Electrical resistivity | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with Electrical resistivity of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 93.5 % Show Material materials with Aluminium of 93.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Copper | 4.5 - 5.2 % Show Material materials with Copper of 4.5 - 5.2 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Iron | 0.18 Show Material materials with Iron of 0.18 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Manganese | 0.001 - 0.5 % Show Material materials with Manganese of 0.001 - 0.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Silicon | 0.18 Show Material materials with Silicon of 0.18 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Titanium | 0.15 - 0.3 % Show Material materials with Titanium of 0.15 - 0.3 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.07 Show Material materials with Zinc of 0.07 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting, sample taken from casting |