EN 1706 Grade AC-43000 T5

Want to keep this datasheet? Save it now in your required format

Description

Aluminium casting alloy (sand casting, permanent mould casting)

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated Standards

Density

20.0 °C

2.65 g/cm³

Show Material materials with Density of 2.65 g/cm³

T5

EN 1706

Mechanical

PropertyTemperatureValueConditionRelated StandardsComment

Elastic modulus

20.0 °C

74.0 GPa

Show Material materials with Elastic modulus of 74.0 GPa

T5

EN 1706

Elongation

-196.0 °C, -120.0 °C, -50.0 °C, 20.0 °C

2.4 %

Show Material materials with Elongation of 2.4 %

T5

EN 1706

20.0 °C

2.2 %

Show Material materials with Elongation of 2.2 %

T5

EN 1706

20.0 °C

2.2 - 2.4 %

Show Material materials with Elongation of 2.2 - 2.4 %

T5

EN 1706

220.0 °C

28.4 %

Show Material materials with Elongation of 28.4 %

T5

EN 1706

280.0 °C

30.1 %

Show Material materials with Elongation of 30.1 %

T5

EN 1706

-196.0 °C

0.6 %

Show Material materials with Elongation of 0.6 %

T5

EN 1706

-120.0 °C

0.5 %

Show Material materials with Elongation of 0.5 %

T5

EN 1706

-50.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

T5

EN 1706

20.0 °C

0.8 %

Show Material materials with Elongation of 0.8 %

T5

EN 1706

220.0 °C

10.6 %

Show Material materials with Elongation of 10.6 %

T5

EN 1706

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Cast 3xx.x Series Aluminium

Shear modulus

2.8 GPa

Show Material materials with Shear modulus of 2.8 GPa

Typical for Cast 3xx.x Series Aluminium

Tensile strength

-196.0 °C, 20.0 °C

304.0 MPa

Show Material materials with Tensile strength of 304.0 MPa

T5

EN 1706

-120.0 °C

275.0 MPa

Show Material materials with Tensile strength of 275.0 MPa

T5

EN 1706

-50.0 °C

263.0 MPa

Show Material materials with Tensile strength of 263.0 MPa

T5

EN 1706

20.0 °C

241.0 MPa

Show Material materials with Tensile strength of 241.0 MPa

T5

EN 1706

20.0 °C

241.0 - 304.0 MPa

Show Material materials with Tensile strength of 241.0 - 304.0 MPa

T5

EN 1706

220.0 °C

68.0 MPa

Show Material materials with Tensile strength of 68.0 MPa

T5

EN 1706

280.0 °C

48.0 MPa

Show Material materials with Tensile strength of 48.0 MPa

T5

EN 1706

-196.0 °C

277.0 MPa

Show Material materials with Tensile strength of 277.0 MPa

T5

EN 1706

-120.0 °C

256.0 MPa

Show Material materials with Tensile strength of 256.0 MPa

T5

EN 1706

-50.0 °C

246.0 MPa

Show Material materials with Tensile strength of 246.0 MPa

T5

EN 1706

20.0 °C

251.0 MPa

Show Material materials with Tensile strength of 251.0 MPa

T5

EN 1706

20.0 °C

235.0 - 251.0 MPa

Show Material materials with Tensile strength of 235.0 - 251.0 MPa

T5

EN 1706

20.0 °C

235.0 MPa

Show Material materials with Tensile strength of 235.0 MPa

T5

EN 1706

220.0 °C

75.0 MPa

Show Material materials with Tensile strength of 75.0 MPa

T5

EN 1706

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

100.0 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T5

EN 1706

Melting point

505.0 - 770.0 °C

Show Material materials with Melting point of 505.0 - 770.0 °C

Typical for Cast 3xx.x Series Aluminium

Specific heat capacity

20.0 °C

910.0 J/(kg·K)

Show Material materials with Specific heat capacity of 910.0 J/(kg·K)

T5

EN 1706

Thermal conductivity

20.0 °C

150.0 - 170.0 W/(m·K)

Show Material materials with Thermal conductivity of 150.0 - 170.0 W/(m·K)

T5

EN 1706

Electrical

PropertyTemperatureValueConditionRelated Standards

Electrical conductivity

20.0 °C

19000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 25000000.0 S/m

T5

EN 1706

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

86.95 %

Show Material materials with Aluminium of 86.95 %

T5

EN 1706

Copper

0.05

Show Material materials with Copper of 0.05

T5

EN 1706

Iron

0.55

Show Material materials with Iron of 0.55

T5

EN 1706

Lead

0.05

Show Material materials with Lead of 0.05

T5

EN 1706

Magnesium

0.2 - 0.45 %

Show Material materials with Magnesium of 0.2 - 0.45 %

T5

EN 1706

Manganese

0.45

Show Material materials with Manganese of 0.45

T5

EN 1706

Nickel

0.05

Show Material materials with Nickel of 0.05

T5

EN 1706

Silicon

9.0 - 11.0 %

Show Material materials with Silicon of 9.0 - 11.0 %

T5

EN 1706

Tin

0.05

Show Material materials with Tin of 0.05

T5

EN 1706

Titanium

0.15

Show Material materials with Titanium of 0.15

T5

EN 1706

Zinc

0.1

Show Material materials with Zinc of 0.1

T5

EN 1706

Technological properties

Property
Processing methods

permanent mould casting