General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 MPa | T6 | WL 3.2134 | Casting | ||
70.0 MPa Show Material materials with Bending Fatigue Strength of 70.0 MPa | T6 | WL 3.2134 | Casting | |||
Elastic modulus | 71.0 GPa Show Material materials with Elastic modulus of 71.0 GPa | T6 | WL 3.2134 | Casting | ||
20.0 °C | 71.0 GPa Show Material materials with Elastic modulus of 71.0 GPa | T6 | WL 3.2134 | |||
Elongation | 0.5 % Show Material materials with Elongation of 0.5 % | T6 | WL 3.2134 | Casting | A50 | |
20.0 °C | 0.5 % Show Material materials with Elongation of 0.5 % | T6 | WL 3.2134 | |||
20.0 °C | 1.5 % Show Material materials with Elongation of 1.5 % | T6 | WL 3.2134 | |||
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | T6 | WL 3.2134 | |||
Hardness, Brinell | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | T6 | WL 3.2134 | Casting | ||
20.0 °C | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | T6 | WL 3.2134 | |||
20.0 °C | 80.0 [-] Show Material materials with Hardness, Brinell of 80.0 [-] | T6 | WL 3.2134 | |||
20.0 °C | 85.0 [-] Show Material materials with Hardness, Brinell of 85.0 [-] | T6 | WL 3.2134 | |||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Shear modulus | 2.8 GPa Show Material materials with Shear modulus of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Shear strength | 20.0 °C | 190.0 MPa Show Material materials with Shear strength of 190.0 MPa | T6 | WL 3.2134 | ||
20.0 °C | 210.0 MPa Show Material materials with Shear strength of 210.0 MPa | T6 | WL 3.2134 | |||
Tensile strength | 190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | T6 | WL 3.2134 | Casting | ||
20.0 °C | 190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | T6 | WL 3.2134 | |||
20.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | T6 | WL 3.2134 | |||
20.0 °C | 210.0 MPa Show Material materials with Tensile strength of 210.0 MPa | T6 | WL 3.2134 | |||
20.0 °C | 220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | T6 | WL 3.2134 | |||
20.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | T6 | WL 3.2134 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | T6 | WL 3.2134 | Casting | |
100 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | T6 | WL 3.2134 | Casting | ||
Melting point | 545.0 - 621.0 °C Show Material materials with Melting point of 545.0 - 621.0 °C | T6 | WL 3.2134 | Casting | ||
Specific heat capacity | 960.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | ||||
Thermal conductivity | 142.0 - 176.0 W/(m·K) Show Material materials with Thermal conductivity of 142.0 - 176.0 W/(m·K) | T6 | WL 3.2134 | Casting |
Electrical
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Electrical conductivity | 19000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 25000000.0 S/m | T6 | WL 3.2134 | Casting |
Electrical resistivity | 4e-08 - 5.26e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 5.26e-08 Ω·m | T6 | WL 3.2134 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.25 % Show Material materials with Chromium of 0.25 % | T6 | WL 3.2134 | Casting |
Copper | 1.0 - 1.5 % Show Material materials with Copper of 1.0 - 1.5 % | T6 | WL 3.2134 | Casting |
Iron | 0.6 % Show Material materials with Iron of 0.6 % | T6 | WL 3.2134 | |
0.60 % Show Material materials with Iron of 0.60 % | T6 | WL 3.2134 | Casting | |
Magnesium | 0.4 - 0.6 % Show Material materials with Magnesium of 0.4 - 0.6 % | T6 | WL 3.2134 | Casting |
Manganese | 0.5 % Show Material materials with Manganese of 0.5 % | T6 | WL 3.2134 | Casting |
Silicon | 4.5 - 5.5 % Show Material materials with Silicon of 4.5 - 5.5 % | T6 | WL 3.2134 | Casting |
Titanium | 0.25 % Show Material materials with Titanium of 0.25 % | T6 | WL 3.2134 | Casting |
Zinc | 0.3 % Show Material materials with Zinc of 0.3 % | T6 | WL 3.2134 | Casting |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting |