Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.6 g/cm³ Show Supplier Material materials with Dichte of 1.6 g/cm³ | dry | ISO 1183 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Biegemodul | 7.6 GPa Show Supplier Material materials with Biegemodul of 7.6 GPa | conditioned | ISO 178 | |||
10.5 GPa Show Supplier Material materials with Biegemodul of 10.5 GPa | dry | ISO 178 | ||||
120 °C | 5.7 GPa Show Supplier Material materials with Biegemodul of 5.7 GPa | dry | ISO 178 | |||
160 °C | 4.7 GPa Show Supplier Material materials with Biegemodul of 4.7 GPa | dry | ISO 178 | |||
Dehnung | 2.4 % Show Supplier Material materials with Dehnung of 2.4 % | dry | ISO 527-1/-2 | 1 mm | ||
2.6 % Show Supplier Material materials with Dehnung of 2.6 % | dry, conditioned | ISO 527-1/-2 | ||||
3.7 % Show Supplier Material materials with Dehnung of 3.7 % | conditioned | ISO 527-1/-2 | ||||
120 °C | 5.8 % Show Supplier Material materials with Dehnung of 5.8 % | dry | ISO 527-1/-2 | |||
160 °C | 6.9 % Show Supplier Material materials with Dehnung of 6.9 % | dry | ISO 527-1/-2 | |||
Elastizitätsmodul | 7.9 GPa Show Supplier Material materials with Elastizitätsmodul of 7.9 GPa | conditioned | ISO 527-1/-2 | |||
8 GPa Show Supplier Material materials with Elastizitätsmodul of 8 GPa | conditioned | ISO 527-1/-2 | ||||
10.5 GPa Show Supplier Material materials with Elastizitätsmodul of 10.5 GPa | dry | ISO 527-1/-2 | 1 mm | |||
11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | dry | ISO 527-1/-2 | ||||
120 °C | 5.5 GPa Show Supplier Material materials with Elastizitätsmodul of 5.5 GPa | dry | ISO 527-1/-2 | |||
160 °C | 4.4 GPa Show Supplier Material materials with Elastizitätsmodul of 4.4 GPa | dry | ISO 527-1/-2 | |||
Flexural yield strength | 185 MPa Show Supplier Material materials with Flexural yield strength of 185 MPa | conditioned | ISO 178 | |||
260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | dry | ISO 178 | ||||
120 °C | 130 MPa Show Supplier Material materials with Flexural yield strength of 130 MPa | dry | ISO 178 | |||
160 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |||
Schlagfestigkeit, Charpy gekerbt | 23 °C | 14.0 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 14.0 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 16 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 16 kJ/m² | conditioned | ISO 179/1eA | |||
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 65 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 65 kJ/m² | dry, conditioned | ISO 179/1eU | ||
Zugfestigkeit | 115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | conditioned | ISO 527-1/-2 | |||
115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | conditioned | ISO 527-1/-2 | at low thickness | |||
160 MPa Show Supplier Material materials with Zugfestigkeit of 160 MPa | dry | ISO 527-1/-2 | ||||
160 MPa Show Supplier Material materials with Zugfestigkeit of 160 MPa | dry | ISO 527-1/-2 | 1 mm | at low thickness | ||
120 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |||
160 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Ball pressure temperature | 250 °C Show Supplier Material materials with Ball pressure temperature of 250 °C | dry | IEC 60695-10-2 | ||
Schmelzpunkt | 260 °C Show Supplier Material materials with Schmelzpunkt of 260 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 235 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 235 °C | dry | ISO 75-1/-2 | 2 MPa | |
260 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 260 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Kriechstromfestigkeit | 300 V Show Supplier Material materials with Kriechstromfestigkeit of 300 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Appliance connector | |
Certifications | Yellow Card Available | |
Fillers | 25% Glass Fiber |