Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.48 g/cm³ Show Supplier Material materials with Densidad of 1.48 g/cm³ | dry | ISO 1183 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | 3.2 % Show Supplier Material materials with Elongación of 3.2 % | dry | ISO 527-1/-2 | |
6 % Show Supplier Material materials with Elongación of 6 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | |
Módulo de flexión | 8.5 GPa Show Supplier Material materials with Módulo de flexión of 8.5 GPa | dry | ISO 178 | |
Módulo elástico | 6 GPa Show Supplier Material materials with Módulo elástico of 6 GPa | conditioned | ISO 527-1/-2 | |
10 GPa Show Supplier Material materials with Módulo elástico of 10 GPa | dry | ISO 527-1/-2 | ||
Resistencia a la tracción | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | conditioned | ISO 527-1/-2 | |
190 MPa Show Supplier Material materials with Resistencia a la tracción of 190 MPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 12.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 16 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 16 kJ/m² | conditioned | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Difusividad térmica | 1.26e-07 mm²/s Show Supplier Material materials with Difusividad térmica of 1.26e-07 mm²/s | dry | - | ||
Temperatura de flexión bajo carga | 290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 2 MPa | |
290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 295 °C Show Supplier Material materials with Temperatura de fusión of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de reblandecimiento Vicat | 290 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 290 °C | dry | ISO 306 | 50°C/h 50N | |
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+07 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+07 Ω·cm | conditioned | IEC 62631-3-1 |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 400 V Show Supplier Material materials with Índice de seguimiento comparativo of 400 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density of melt | 1320 g/cm³ Show Supplier Material materials with Density of melt of 1320 g/cm³ | dry | - |
Specific heat capacity melt | 1890 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1890 J/(kg·K) | dry | - |
Thermal conductivity of melt | 0.319 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.319 W/(m·K) | dry | - |
Viscosity number | 145 cm³/gr Show Supplier Material materials with Viscosity number of 145 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Fillers | 30% Glass Fiber and PTFE |