Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.6 g/cm³ Show Supplier Material materials with Densidad of 1.6 g/cm³ | dry | ISO 1183 |
Mecánica
Property | Temperature | Value | Condition | Thickness | Testing Standard | Comment |
---|---|---|---|---|---|---|
Elongación | 2.4 % Show Supplier Material materials with Elongación of 2.4 % | dry | 1 mm | ISO 527-1/-2 | ||
2.6 % Show Supplier Material materials with Elongación of 2.6 % | dry, conditioned | ISO 527-1/-2 | ||||
3.7 % Show Supplier Material materials with Elongación of 3.7 % | conditioned | ISO 527-1/-2 | ||||
120 °C | 5.8 % Show Supplier Material materials with Elongación of 5.8 % | dry | ISO 527-1/-2 | |||
160 °C | 6.9 % Show Supplier Material materials with Elongación of 6.9 % | dry | ISO 527-1/-2 | |||
Flexural yield strength | 185 MPa Show Supplier Material materials with Flexural yield strength of 185 MPa | conditioned | ISO 178 | |||
260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | dry | ISO 178 | ||||
120 °C | 130 MPa Show Supplier Material materials with Flexural yield strength of 130 MPa | dry | ISO 178 | |||
160 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |||
Módulo de flexión | 7.6 GPa Show Supplier Material materials with Módulo de flexión of 7.6 GPa | conditioned | ISO 178 | |||
10.5 GPa Show Supplier Material materials with Módulo de flexión of 10.5 GPa | dry | ISO 178 | ||||
120 °C | 5.7 GPa Show Supplier Material materials with Módulo de flexión of 5.7 GPa | dry | ISO 178 | |||
160 °C | 4.7 GPa Show Supplier Material materials with Módulo de flexión of 4.7 GPa | dry | ISO 178 | |||
Módulo elástico | 7.9 GPa Show Supplier Material materials with Módulo elástico of 7.9 GPa | conditioned | ISO 527-1/-2 | |||
8 GPa Show Supplier Material materials with Módulo elástico of 8 GPa | conditioned | ISO 527-1/-2 | ||||
10.5 GPa Show Supplier Material materials with Módulo elástico of 10.5 GPa | dry | 1 mm | ISO 527-1/-2 | |||
11 GPa Show Supplier Material materials with Módulo elástico of 11 GPa | dry | ISO 527-1/-2 | ||||
120 °C | 5.5 GPa Show Supplier Material materials with Módulo elástico of 5.5 GPa | dry | ISO 527-1/-2 | |||
160 °C | 4.4 GPa Show Supplier Material materials with Módulo elástico of 4.4 GPa | dry | ISO 527-1/-2 | |||
Resistencia a la tracción | 115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | conditioned | ISO 527-1/-2 | |||
115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | conditioned | ISO 527-1/-2 | at low thickness | |||
160 MPa Show Supplier Material materials with Resistencia a la tracción of 160 MPa | dry | ISO 527-1/-2 | ||||
160 MPa Show Supplier Material materials with Resistencia a la tracción of 160 MPa | dry | 1 mm | ISO 527-1/-2 | at low thickness | ||
120 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |||
160 °C | 70 MPa Show Supplier Material materials with Resistencia a la tracción of 70 MPa | dry | ISO 527-1/-2 | |||
Resistencia al choque, ensayo Charpy entallado | 23 °C | 14.0 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 14.0 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 16 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 16 kJ/m² | conditioned | ISO 179/1eA | |||
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | dry, conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Ball pressure temperature | 250 °C Show Supplier Material materials with Ball pressure temperature of 250 °C | dry | IEC 60695-10-2 | ||
Temperatura de flexión bajo carga | 235 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 235 °C | dry | ISO 75-1/-2 | 2 MPa | |
260 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 260 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 260 °C Show Supplier Material materials with Temperatura de fusión of 260 °C | dry | ISO 11357-1/-3 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Índice de seguimiento comparativo | 300 V Show Supplier Material materials with Índice de seguimiento comparativo of 300 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Appliance connector | |
Certifications | Yellow Card Available | |
Fillers | 25% Glass Fiber |