Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 0.3 % Show Supplier Material materials with Absorción de agua of 0.3 % | dry | ISO 62 | at 23°C after 24h |
4 % Show Supplier Material materials with Absorción de agua of 4 % | dry | Sim. to ISO 62 | ||
Densidad | 1.65 g/cm³ Show Supplier Material materials with Densidad of 1.65 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 2 % Show Supplier Material materials with Elongación of 2 % | dry, conditioned | ISO 527-1/-2 |
2 % Show Supplier Material materials with Elongación of 2 % | conditioned | ISO 527-1/-2 | ||
2.1 % Show Supplier Material materials with Elongación of 2.1 % | dry | ISO 527-1/-2 | ||
40 °C | 2.1 % Show Supplier Material materials with Elongación of 2.1 % | dry, conditioned | ISO 527-1/-2 | |
80 °C | 2.3 % Show Supplier Material materials with Elongación of 2.3 % | dry | ISO 527-1/-2 | |
80 °C | 4 % Show Supplier Material materials with Elongación of 4 % | conditioned | ISO 527-1/-2 | |
100 °C | 2.6 % Show Supplier Material materials with Elongación of 2.6 % | dry | ISO 527-1/-2 | |
100 °C | 4.5 % Show Supplier Material materials with Elongación of 4.5 % | conditioned | ISO 527-1/-2 | |
120 °C | 3.6 % Show Supplier Material materials with Elongación of 3.6 % | dry | ISO 527-1/-2 | |
120 °C | 5.5 % Show Supplier Material materials with Elongación of 5.5 % | conditioned | ISO 527-1/-2 | |
150 °C | 5.7 % Show Supplier Material materials with Elongación of 5.7 % | dry | ISO 527-1/-2 | |
160 °C | 6 % Show Supplier Material materials with Elongación of 6 % | dry | ISO 527-1/-2 | |
180 °C | 6 % Show Supplier Material materials with Elongación of 6 % | dry | ISO 527-1/-2 | |
200 °C | 6 % Show Supplier Material materials with Elongación of 6 % | dry | ISO 527-1/-2 | |
210 °C | 0.006 % Show Supplier Material materials with Elongación of 0.006 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 310 MPa Show Supplier Material materials with Flexural yield strength of 310 MPa | conditioned | ISO 178 | |
390 MPa Show Supplier Material materials with Flexural yield strength of 390 MPa | dry | ISO 178 | ||
120 °C | 210 MPa Show Supplier Material materials with Flexural yield strength of 210 MPa | dry | ISO 178 | |
160 °C | 150 MPa Show Supplier Material materials with Flexural yield strength of 150 MPa | dry | ISO 178 | |
180 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
200 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
210 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |
Módulo de flexión | 17.3 GPa Show Supplier Material materials with Módulo de flexión of 17.3 GPa | dry | ISO 178 | |
17.8 GPa Show Supplier Material materials with Módulo de flexión of 17.8 GPa | conditioned | ISO 178 | ||
120 °C | 11.7 GPa Show Supplier Material materials with Módulo de flexión of 11.7 GPa | dry | ISO 178 | |
160 °C | 7.5 GPa Show Supplier Material materials with Módulo de flexión of 7.5 GPa | dry | ISO 178 | |
180 °C | 6.4 GPa Show Supplier Material materials with Módulo de flexión of 6.4 GPa | dry | ISO 178 | |
200 °C | 6 GPa Show Supplier Material materials with Módulo de flexión of 6 GPa | dry | ISO 178 | |
210 °C | 5.9 GPa Show Supplier Material materials with Módulo de flexión of 5.9 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 18.3 GPa Show Supplier Material materials with Módulo elástico of 18.3 GPa | dry | ISO 527-1/-2 |
-40 °C | 18.5 GPa Show Supplier Material materials with Módulo elástico of 18.5 GPa | conditioned | ISO 527-1/-2 | |
18 GPa Show Supplier Material materials with Módulo elástico of 18 GPa | dry | ISO 527-1/-2 | ||
18.3 GPa Show Supplier Material materials with Módulo elástico of 18.3 GPa | conditioned | ISO 527-1/-2 | ||
40 °C | 17.2 GPa Show Supplier Material materials with Módulo elástico of 17.2 GPa | conditioned | ISO 527-1/-2 | |
40 °C | 17.6 GPa Show Supplier Material materials with Módulo elástico of 17.6 GPa | dry | ISO 527-1/-2 | |
80 °C | 10.9 GPa Show Supplier Material materials with Módulo elástico of 10.9 GPa | conditioned | ISO 527-1/-2 | |
80 °C | 16.8 GPa Show Supplier Material materials with Módulo elástico of 16.8 GPa | dry | ISO 527-1/-2 | |
100 °C | 8.7 GPa Show Supplier Material materials with Módulo elástico of 8.7 GPa | conditioned | ISO 527-1/-2 | |
100 °C | 15.7 GPa Show Supplier Material materials with Módulo elástico of 15.7 GPa | dry | ISO 527-1/-2 | |
120 °C | 7.7 GPa Show Supplier Material materials with Módulo elástico of 7.7 GPa | conditioned | ISO 527-1/-2 | |
120 °C | 12.4 GPa Show Supplier Material materials with Módulo elástico of 12.4 GPa | dry | ISO 527-1/-2 | |
150 °C | 8.2 GPa Show Supplier Material materials with Módulo elástico of 8.2 GPa | dry | ISO 527-1/-2 | |
160 °C | 7.7 GPa Show Supplier Material materials with Módulo elástico of 7.7 GPa | dry | ISO 527-1/-2 | |
180 °C | 7.1 GPa Show Supplier Material materials with Módulo elástico of 7.1 GPa | dry | ISO 527-1/-2 | |
200 °C | 6.8 GPa Show Supplier Material materials with Módulo elástico of 6.8 GPa | dry | ISO 527-1/-2 | |
210 °C | 6.3 GPa Show Supplier Material materials with Módulo elástico of 6.3 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 280 MPa Show Supplier Material materials with Resistencia a la tracción of 280 MPa | dry | ISO 527-1/-2 |
-40 °C | 290 MPa Show Supplier Material materials with Resistencia a la tracción of 290 MPa | conditioned | ISO 527-1/-2 | |
240 MPa Show Supplier Material materials with Resistencia a la tracción of 240 MPa | conditioned | ISO 527-1/-2 | ||
260 MPa Show Supplier Material materials with Resistencia a la tracción of 260 MPa | dry | ISO 527-1/-2 | ||
40 °C | 220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | conditioned | ISO 527-1/-2 | |
40 °C | 250 MPa Show Supplier Material materials with Resistencia a la tracción of 250 MPa | dry | ISO 527-1/-2 | |
80 °C | 140 MPa Show Supplier Material materials with Resistencia a la tracción of 140 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | dry | ISO 527-1/-2 | |
100 °C | 115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | conditioned | ISO 527-1/-2 | |
100 °C | 195 MPa Show Supplier Material materials with Resistencia a la tracción of 195 MPa | dry | ISO 527-1/-2 | |
120 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | conditioned | ISO 527-1/-2 | |
120 °C | 155 MPa Show Supplier Material materials with Resistencia a la tracción of 155 MPa | dry | ISO 527-1/-2 | |
150 °C | 115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | dry | ISO 527-1/-2 | |
160 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | dry | ISO 527-1/-2 | |
180 °C | 90 MPa Show Supplier Material materials with Resistencia a la tracción of 90 MPa | dry | ISO 527-1/-2 | |
200 °C | 82 MPa Show Supplier Material materials with Resistencia a la tracción of 82 MPa | dry | ISO 527-1/-2 | |
210 °C | 76 MPa Show Supplier Material materials with Resistencia a la tracción of 76 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry | ISO 179/1eA | |
23 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | dry | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 80 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2.7e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.7e-07 1/K | dry | ASTM D696 | Parallel | |
3e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3e-07 1/K | dry | ASTM D696 | Normal | ||
Temperatura de flexión bajo carga | 305 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 305 °C | dry | ISO 75-1/-2 | 2 MPa | |
318 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 318 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 325 °C Show Supplier Material materials with Temperatura de fusión of 325 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | 125 °C Show Supplier Material materials with Temperatura de transición del vidrio of 125 °C | dry | ISO 11357-1/-2 | 10°C/min | |
130 °C Show Supplier Material materials with Temperatura de transición del vidrio of 130 °C | dry | ASTM D5026/D7028 | DMTA (tan d) |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4.8 [-] Show Supplier Material materials with Constante dieléctrica of 4.8 [-] | dry | IEC 62631-2-1 | 1MHz |
5 [-] Show Supplier Material materials with Constante dieléctrica of 5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
5.1 [-] Show Supplier Material materials with Constante dieléctrica of 5.1 [-] | dry | IEC 62631-2-1 | 100Hz | |
5.8 [-] Show Supplier Material materials with Constante dieléctrica of 5.8 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 54 [-] Show Supplier Material materials with Factor de disipación of 54 [-] | dry | IEC 62631-2-1 | 100Hz |
160 [-] Show Supplier Material materials with Factor de disipación of 160 [-] | dry | IEC 62631-2-1 | 1MHz | |
270 [-] Show Supplier Material materials with Factor de disipación of 270 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
280 [-] Show Supplier Material materials with Factor de disipación of 280 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 | |
Índice de seguimiento comparativo | 425 V Show Supplier Material materials with Índice de seguimiento comparativo of 425 V | dry | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Crankshaft Covers | |
Certifications | Yellow Card Available | |
Fillers | 50% Glass Fiber |